General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.66 g/cm³ Show Supplier Material materials with Density of 1.66 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 8.7 GPa Show Supplier Material materials with Elastic modulus of 8.7 GPa | conditioned | ISO 527-1/-2 | |
12.1 GPa Show Supplier Material materials with Elastic modulus of 12.1 GPa | dry | ISO 527-1/-2 | ||
Elongation | 1.7 % Show Supplier Material materials with Elongation of 1.7 % | dry | ISO 527-1/-2 | |
2.5 % Show Supplier Material materials with Elongation of 2.5 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 8.6 GPa Show Supplier Material materials with Flexural modulus of 8.6 GPa | conditioned | ISO 178 | |
11.5 GPa Show Supplier Material materials with Flexural modulus of 11.5 GPa | dry | ISO 178 | ||
Flexural yield strength | 210 MPa Show Supplier Material materials with Flexural yield strength of 210 MPa | conditioned | ISO 178 | |
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||
Impact strength, Charpy notched | 23 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | dry | ISO 179/1eA |
23 °C | 14.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 14.0 kJ/m² | conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | 23 °C | 54 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 54 kJ/m² | dry | ISO 179/1eU |
23 °C | 64 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 64 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | 130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | conditioned | ISO 527-1/-2 | |
160 MPa Show Supplier Material materials with Tensile strength of 160 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
Heat deflection temperature | 213 °C Show Supplier Material materials with Heat deflection temperature of 213 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 225 V Show Supplier Material materials with Comparative tracking index of 225 V | dry | IEC 60112 | |
Dielectric constant | 4 [-] Show Supplier Material materials with Dielectric constant of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
5 [-] Show Supplier Material materials with Dielectric constant of 5 [-] | dry | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 23 kV/mm Show Supplier Material materials with Dielectric strength of 23 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 130 [-] Show Supplier Material materials with Dissipation factor of 130 [-] | dry | IEC 62631-2-1 | 100Hz |
190 [-] Show Supplier Material materials with Dissipation factor of 190 [-] | dry | IEC 62631-2-1 | 1MHz | |
Surface resistivity | 6e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 6e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 6e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 6e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt mass-flow rate | 250 °C | 41 g/10min Show Supplier Material materials with Melt mass-flow rate of 41 g/10min | dry | ISO 1133 | |
Melt volume-flow rate | 250 °C | 31 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 31 cm³/10min | dry | ISO 1133 | |
Shrinkage | 0.2 % Show Supplier Material materials with Shrinkage of 0.2 % | dry | ISO 294-4 | Parallel | |
0.9 % Show Supplier Material materials with Shrinkage of 0.9 % | dry | ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Fillers | 30% Glass Fiber |