General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.47 g/cm³ Show Supplier Material materials with Density of 1.47 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 | |
Water absorption | 1.7 % Show Supplier Material materials with Water absorption of 1.7 % | dry | ISO 62 | at 23°C after 24h |
6.7 % Show Supplier Material materials with Water absorption of 6.7 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 8 GPa Show Supplier Material materials with Elastic modulus of 8 GPa | conditioned | ISO 527-1/-2 | |||
12.5 GPa Show Supplier Material materials with Elastic modulus of 12.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
12.5 GPa Show Supplier Material materials with Elastic modulus of 12.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
Elongation | 1.9 % Show Supplier Material materials with Elongation of 1.9 % | dry | ISO 527-1/-2 | 1 mm | ||
2.3 % Show Supplier Material materials with Elongation of 2.3 % | dry | ISO 527-1/-2 | 1 mm | |||
3.5 % Show Supplier Material materials with Elongation of 3.5 % | conditioned | ISO 527-1/-2 | ||||
Flexural modulus | 8.5 GPa Show Supplier Material materials with Flexural modulus of 8.5 GPa | conditioned | ISO 178 | |||
12 GPa Show Supplier Material materials with Flexural modulus of 12 GPa | dry | ISO 178 | ||||
Flexural yield strength | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | conditioned | ISO 178 | |||
270 MPa Show Supplier Material materials with Flexural yield strength of 270 MPa | dry | ISO 178 | ||||
Impact strength, Charpy notched | 23 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | conditioned | ISO 179/1eA | |||
Impact strength, Charpy unnotched | 23 °C | 60 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 60 kJ/m² | dry | ISO 179/1eU | ||
23 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | conditioned | ISO 179/1eU | |||
Tensile strength | 130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | conditioned | ISO 527-1/-2 | |||
185 MPa Show Supplier Material materials with Tensile strength of 185 MPa | dry | ISO 527-1/-2 | 1 mm | |||
200 MPa Show Supplier Material materials with Tensile strength of 200 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 4e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 4e-07 1/K | dry | ASTM D696 | Parallel | ||
4.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 4.5e-07 1/K | dry | ASTM D696 | Normal | |||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
Glow Wire Ignition Temperature | 825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | IEC 60695-2-13 | 3 mm | ||
Heat deflection temperature | 280 °C Show Supplier Material materials with Heat deflection temperature of 280 °C | dry | ISO 75-1/-2 | 2 MPa | ||
285 °C Show Supplier Material materials with Heat deflection temperature of 285 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 280 °C Show Supplier Material materials with Melting point of 280 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Comparative tracking index | 425 V Show Supplier Material materials with Comparative tracking index of 425 V | dry | IEC 60112 |
Surface resistivity | 1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available | |
Fillers | 35% Glass Fiber |