General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.26 g/cm³ Show Supplier Material materials with Density of 1.26 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 3 % Show Supplier Material materials with Moisture absorption of 3 % | dry | Sim. to ISO 62 | |
Water absorption | 3.1 % Show Supplier Material materials with Water absorption of 3.1 % | dry | ISO 62 | at 23°C after 24h |
11.3 % Show Supplier Material materials with Water absorption of 11.3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 2.8 GPa Show Supplier Material materials with Elastic modulus of 2.8 GPa | dry | ISO 527-1/-2 | |
Elongation | 20 % Show Supplier Material materials with Elongation of 20 % | dry | ISO 527-1/-2 | |
Flexural modulus | 2.4 GPa Show Supplier Material materials with Flexural modulus of 2.4 GPa | dry | ISO 178 | |
Flexural yield strength | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | 23 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m² | dry | ISO 179/1eA |
Tensile strength | 80 MPa Show Supplier Material materials with Tensile strength of 80 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Heat deflection temperature | 160 °C Show Supplier Material materials with Heat deflection temperature of 160 °C | dry | ISO 75-1/-2 | 2 MPa | |
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Front End Accessory Drive Parts: Belt Tensioner,Damping bands, Shoes and Bushings | |
Fillers | Aramid Fiber |