General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.56 g/cm³ Show Supplier Material materials with Density of 1.56 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.2 % Show Supplier Material materials with Moisture absorption of 1.2 % | dry | Sim. to ISO 62 |
Water absorption | 3 % Show Supplier Material materials with Water absorption of 3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 16 GPa Show Supplier Material materials with Elastic modulus of 16 GPa | conditioned | ISO 527-1/-2 | |
16.5 GPa Show Supplier Material materials with Elastic modulus of 16.5 GPa | dry | ISO 527-1/-2 | ||
120 °C | 4.9 GPa Show Supplier Material materials with Elastic modulus of 4.9 GPa | dry | ISO 527-1/-2 | |
140 °C | 4.5 GPa Show Supplier Material materials with Elastic modulus of 4.5 GPa | dry | ISO 527-1/-2 | |
160 °C | 4 GPa Show Supplier Material materials with Elastic modulus of 4 GPa | dry | ISO 527-1/-2 | |
Elongation | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
3.3 % Show Supplier Material materials with Elongation of 3.3 % | conditioned | ISO 527-1/-2 | ||
120 °C | 12 % Show Supplier Material materials with Elongation of 12 % | dry | ISO 527-1/-2 | |
140 °C | 11 % Show Supplier Material materials with Elongation of 11 % | dry | ISO 527-1/-2 | |
160 °C | 10 % Show Supplier Material materials with Elongation of 10 % | dry | ISO 527-1/-2 | |
Flexural modulus | 15 GPa Show Supplier Material materials with Flexural modulus of 15 GPa | conditioned | ISO 178 | |
15.5 GPa Show Supplier Material materials with Flexural modulus of 15.5 GPa | dry | ISO 178 | ||
Flexural yield strength | 330 MPa Show Supplier Material materials with Flexural yield strength of 330 MPa | conditioned | ISO 178 | |
380 MPa Show Supplier Material materials with Flexural yield strength of 380 MPa | dry | ISO 178 | ||
Impact strength, Charpy notched | -30 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 14.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 14.0 kJ/m² | dry | ISO 179/1eA | |
23 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 16 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 75 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 80 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 100 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | 210 MPa Show Supplier Material materials with Tensile strength of 210 MPa | conditioned | ISO 527-1/-2 | |
240 MPa Show Supplier Material materials with Tensile strength of 240 MPa | dry | ISO 527-1/-2 | ||
120 °C | 75 MPa Show Supplier Material materials with Tensile strength of 75 MPa | dry | ISO 527-1/-2 | |
140 °C | 60 MPa Show Supplier Material materials with Tensile strength of 60 MPa | dry | ISO 527-1/-2 | |
160 °C | 50 MPa Show Supplier Material materials with Tensile strength of 50 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1e-06 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | HB | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glass transition temperature | 88 °C Show Supplier Material materials with Glass transition temperature of 88 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Heat deflection temperature | 200 °C Show Supplier Material materials with Heat deflection temperature of 200 °C | dry | ISO 75-1/-2 | 2 MPa | ||
235 °C Show Supplier Material materials with Heat deflection temperature of 235 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 250 °C Show Supplier Material materials with Melting point of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dielectric strength | 27 kV/mm Show Supplier Material materials with Dielectric strength of 27 kV/mm | dry | IEC 60243-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Faucet mixing valve, Pump Housings, Faucet system components, Bakeware | |
Certifications | Food Contact, Drinking Water, Yellow Card Available | |
Fillers | 50% Glass Fiber |