General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 71 % Show Supplier Material materials with Bio-based content of 71 % | dry | ASTM D6866-12 Method B |
Density | 1.2 g/cm³ Show Supplier Material materials with Density of 1.2 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 3.8 GPa Show Supplier Material materials with Elastic modulus of 3.8 GPa | conditioned | ISO 527-1/-2 | |
5.6 GPa Show Supplier Material materials with Elastic modulus of 5.6 GPa | dry | ISO 527-1/-2 | ||
Elongation | 3.5 % Show Supplier Material materials with Elongation of 3.5 % | dry | ISO 527-1/-2 | |
6.5 % Show Supplier Material materials with Elongation of 6.5 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 5 GPa Show Supplier Material materials with Flexural modulus of 5 GPa | dry | ISO 178 | |
Flexural yield strength | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | 23 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m² | dry | ISO 179/1eA |
Impact strength, Charpy unnotched | 23 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | dry | ISO 179/1eU |
Tensile strength | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | conditioned | ISO 527-1/-2 | |
125 MPa Show Supplier Material materials with Tensile strength of 125 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Heat deflection temperature | 214 °C Show Supplier Material materials with Heat deflection temperature of 214 °C | dry | ISO 75-1/-2 | 2 MPa | |
242 °C Show Supplier Material materials with Heat deflection temperature of 242 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 250 °C Show Supplier Material materials with Melting point of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Technological properties
Property | ||
---|---|---|
Certifications | Food Contact | |
Fillers | 15% Glass Fiber |