General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.76 g/cm³ Show Supplier Material materials with Density of 1.76 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 | |
Water absorption | 1.5 % Show Supplier Material materials with Water absorption of 1.5 % | dry | ISO 62 | at 23°C after 24h |
5.4 % Show Supplier Material materials with Water absorption of 5.4 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 23 GPa Show Supplier Material materials with Elastic modulus of 23 GPa | dry | ISO 527-1/-2 |
12 GPa Show Supplier Material materials with Elastic modulus of 12 GPa | conditioned | ISO 527-1/-2 | ||
20 GPa Show Supplier Material materials with Elastic modulus of 20 GPa | dry | ISO 527-1/-2 | ||
120 °C | 10 GPa Show Supplier Material materials with Elastic modulus of 10 GPa | dry | ISO 527-1/-2 | |
160 °C | 9.1 GPa Show Supplier Material materials with Elastic modulus of 9.1 GPa | dry | ISO 527-1/-2 | |
180 °C | 8.5 GPa Show Supplier Material materials with Elastic modulus of 8.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 8 GPa Show Supplier Material materials with Elastic modulus of 8 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 1.6 % Show Supplier Material materials with Elongation of 1.6 % | dry | ISO 527-1/-2 |
2 % Show Supplier Material materials with Elongation of 2 % | dry | ISO 527-1/-2 | ||
3 % Show Supplier Material materials with Elongation of 3 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
160 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
180 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
200 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
Flexural modulus | 10 GPa Show Supplier Material materials with Flexural modulus of 10 GPa | conditioned | ISO 178 | |
17 GPa Show Supplier Material materials with Flexural modulus of 17 GPa | dry | ISO 178 | ||
Impact strength, Charpy notched | -30 °C | 18 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 18 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 18 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 18 kJ/m² | dry, conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 65 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 65 kJ/m² | dry | ISO 179/1eU |
-30 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 75 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 90 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 100 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | -40 °C | 250 MPa Show Supplier Material materials with Tensile strength of 250 MPa | dry | ISO 527-1/-2 |
170 MPa Show Supplier Material materials with Tensile strength of 170 MPa | conditioned | ISO 527-1/-2 | ||
255 MPa Show Supplier Material materials with Tensile strength of 255 MPa | dry | ISO 527-1/-2 | ||
120 °C | 150 MPa Show Supplier Material materials with Tensile strength of 150 MPa | dry | ISO 527-1/-2 | |
160 °C | 125 MPa Show Supplier Material materials with Tensile strength of 125 MPa | dry | ISO 527-1/-2 | |
180 °C | 110 MPa Show Supplier Material materials with Tensile strength of 110 MPa | dry | ISO 527-1/-2 | |
200 °C | 100 MPa Show Supplier Material materials with Tensile strength of 100 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
3.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | |
290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Thermal diffusivity | 1.94e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 1.94e-07 mm²/s | dry | - | ||
Vicat softening temperature | 290 °C Show Supplier Material materials with Vicat softening temperature of 290 °C | dry | ISO 306 | 50°C/h 50N |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1550 g/cm³ Show Supplier Material materials with Density of melt of 1550 g/cm³ | dry | - | |
Shrinkage | 0.4 % Show Supplier Material materials with Shrinkage of 0.4 % | dry | ISO 294-4 | Parallel |
0.7 % Show Supplier Material materials with Shrinkage of 0.7 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 1450 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1450 J/(kg·K) | dry | - | |
Spiral flow length | 110 | dry | - | 1.0 mm 800 bar |
125 | dry | - | 1.0 mm 900 bar | |
140 | dry | - | 1.0 mm 1000 bar | |
Thermal conductivity of melt | 0.43 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.43 W/(m·K) | dry | - | |
Viscosity number | 75 cm³/gr Show Supplier Material materials with Viscosity number of 75 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Tractor Engine Transmission Components, Torque Convertor Components, Gears, Timing drive systems, Electronic throttle control actuators, Exhaust gas recirculation actuators, Turbo actuators, Coolant valve actuators | |
Certifications | Yellow Card Available | |
Fillers | 60% Glass Fiber |