General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.08 g/cm³ Show Supplier Material materials with Density of 1.08 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.9 % Show Supplier Material materials with Moisture absorption of 2.9 % | dry | Sim. to ISO 62 |
Water absorption | 7.4 % Show Supplier Material materials with Water absorption of 7.4 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 2.3 GPa Show Supplier Material materials with Elastic modulus of 2.3 GPa | dry | ISO 527-1/-2 |
0.55 GPa Show Supplier Material materials with Elastic modulus of 0.55 GPa | conditioned | ISO 527-1/-2 | ||
2.1 GPa Show Supplier Material materials with Elastic modulus of 2.1 GPa | dry | ISO 527-1/-2 | ||
Elongation | -40 °C | 18 % Show Supplier Material materials with Elongation of 18 % | dry | ISO 527-1/-2 |
50 % Show Supplier Material materials with Elongation of 50 % | dry, conditioned | ISO 527-1/-2 | ||
Elongation at yield | -40 °C | 7.5 % Show Supplier Material materials with Elongation at yield of 7.5 % | dry | ISO 527-1/-2 |
4 % Show Supplier Material materials with Elongation at yield of 4 % | dry | ISO 527-1/-2 | ||
Flexural modulus | 0.52 GPa Show Supplier Material materials with Flexural modulus of 0.52 GPa | conditioned | ISO 178 | |
2 GPa Show Supplier Material materials with Flexural modulus of 2 GPa | dry | ISO 178 | ||
Flexural yield strength | 22 MPa Show Supplier Material materials with Flexural yield strength of 22 MPa | conditioned | ISO 178 | |
75 MPa Show Supplier Material materials with Flexural yield strength of 75 MPa | dry | ISO 178 | ||
Impact strength, Charpy notched | -30 °C | 21 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 21 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 22 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 22 kJ/m² | dry | ISO 179/1eA | |
23 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 90 kJ/m² | dry | ISO 179/1eA | |
Puncture energy | -40 °C | 75 J Show Supplier Material materials with Puncture energy of 75 J | dry | ISO 6603-2 |
-30 °C | 63 J Show Supplier Material materials with Puncture energy of 63 J | dry | ISO 6603-2 | |
23 °C | 49 J Show Supplier Material materials with Puncture energy of 49 J | dry | ISO 6603-2 | |
Puncture force | -40 °C | 5800 N Show Supplier Material materials with Puncture force of 5800 N | dry | ISO 6603-2 |
-30 °C | 5500 N Show Supplier Material materials with Puncture force of 5500 N | dry | ISO 6603-2 | |
23 °C | 4000 N Show Supplier Material materials with Puncture force of 4000 N | dry | ISO 6603-2 | |
Tensile strength | -40 °C | 60 MPa Show Supplier Material materials with Tensile strength of 60 MPa | dry | ISO 527-1/-2 |
46 MPa Show Supplier Material materials with Tensile strength of 46 MPa | dry | ISO 527-1/-2 | ||
Yield strength | -40 °C | 84 MPa Show Supplier Material materials with Yield strength of 84 MPa | dry | ISO 527-1/-2 |
58.0 MPa Show Supplier Material materials with Yield strength of 58.0 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 9e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 9e-07 1/K | dry | ISO 11359-1/-2 | Normal | |
1.5e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.5e-06 1/K | dry | ISO 11359-1/-2 | Parallel | ||
Glass transition temperature | 71 °C Show Supplier Material materials with Glass transition temperature of 71 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | |
Heat deflection temperature | 55 °C Show Supplier Material materials with Heat deflection temperature of 55 °C | dry | ISO 75-1/-2 | 2 MPa | |
100 °C Show Supplier Material materials with Heat deflection temperature of 100 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Vicat softening temperature | 155 °C Show Supplier Material materials with Vicat softening temperature of 155 °C | dry | ISO 306 | 50°C/h 50N |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt volume-flow rate | 275 °C | 35 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 35 cm³/10min | dry | ISO 1133 | |
Shrinkage | 1.5 % Show Supplier Material materials with Shrinkage of 1.5 % | dry | ISO 294-4 | Normal | |
1.6 % Show Supplier Material materials with Shrinkage of 1.6 % | dry | ISO 294-4 | Parallel |
Technological properties
Property | ||
---|---|---|
Application areas | Gasoline Tank in hybrid cars |