General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Coefficient of friction, kinetic | 1 [-] Show Supplier Material materials with Coefficient of friction, kinetic of 1 [-] | dry | ISO 8295 |
Coefficient of friction, static | 1.2 [-] Show Supplier Material materials with Coefficient of friction, static of 1.2 [-] | dry | ISO 8295 |
Density | 1.13 g/cm³ Show Supplier Material materials with Density of 1.13 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.8 % Show Supplier Material materials with Moisture absorption of 2.8 % | dry | Sim. to ISO 62 |
Water absorption | 9 % Show Supplier Material materials with Water absorption of 9 % | dry | Sim. to ISO 62 |
Mechanical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Elastic modulus | 0.46 GPa Show Supplier Material materials with Elastic modulus of 0.46 GPa | dry | DSM-Method, 50 mm/min | |
Elongation | 350 % Show Supplier Material materials with Elongation of 350 % | dry | ISO 527-3 | Parallel |
Tensile strength | 82 MPa Show Supplier Material materials with Tensile strength of 82 MPa | dry | ISO 527-3 | Parallel |
Yield strength | 31 MPa Show Supplier Material materials with Yield strength of 31 MPa | dry | ISO 527-3 | Parallel |
Thermal
Optical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Transparency | 83 | dry | DSM method |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Melt viscosity | 260 °C | 810 Pa·s Show Supplier Material materials with Melt viscosity of 810 Pa·s | dry | DSM method, 260 °C |
Viscosity number | 196 cm³/gr Show Supplier Material materials with Viscosity number of 196 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Certifications | Food Contact |