General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.56 g/cm³ Show Supplier Material materials with Density of 1.56 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.6 % Show Supplier Material materials with Moisture absorption of 1.6 % | dry | Sim. to ISO 62 |
Water absorption | 4.2 % Show Supplier Material materials with Water absorption of 4.2 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 16 GPa Show Supplier Material materials with Elastic modulus of 16 GPa | dry | ISO 527-1/-2 | |
Elongation | 2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | ISO 527-1/-2 | |
Impact strength, Charpy notched | 23 °C | 18 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 18 kJ/m² | dry | ISO 179/1eA |
Tensile strength | 260 MPa Show Supplier Material materials with Tensile strength of 260 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Thickness | Comment |
---|---|---|---|---|---|---|
Heat deflection temperature | 245 °C Show Supplier Material materials with Heat deflection temperature of 245 °C | dry | ISO 75-1/-2 | 2 MPa | ||
Melting point | 315 °C Show Supplier Material materials with Melting point of 315 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 85 °C Show Supplier Material materials with Relative temperature index, electrical of 85 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 85 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 85 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 85 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 85 °C | dry | UL746B | 0.75 mm |
Electrical
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 50% Glass Fiber |