General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.28 g/cm³ Show Supplier Material materials with Density of 1.28 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.25 % Show Supplier Material materials with Moisture absorption of 0.25 % | dry | Sim. to ISO 62 |
Water absorption | 0.6 % Show Supplier Material materials with Water absorption of 0.6 % | dry | Sim. to ISO 62 |
Mechanical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Elastic modulus | 0.25 GPa Show Supplier Material materials with Elastic modulus of 0.25 GPa | dry | ISO 527-1/-2 | |
Elongation | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | |
Elongation at yield | 22 % Show Supplier Material materials with Elongation at yield of 22 % | dry | ISO 527-1/-2 | |
Hardness, Shore D | 55.0 [-] Show Supplier Material materials with Hardness, Shore D of 55.0 [-] | dry | ISO 868 | 3s |
55.0 [-] Show Supplier Material materials with Hardness, Shore D of 55.0 [-] | dry | ISO 868 | 15s | |
Tensile strength | 27 MPa Show Supplier Material materials with Tensile strength of 27 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Thickness | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|---|
Flammability | V-2 | dry | 1.5 mm | IEC 60695-11-10 | UL recognition :Yes | |
Heat deflection temperature | 85 °C Show Supplier Material materials with Heat deflection temperature of 85 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 200 °C Show Supplier Material materials with Melting point of 200 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 50 °C Show Supplier Material materials with Relative temperature index, electrical of 50 °C | dry | 2 mm | UL746B | ||
Relative temperature index, mechanical impact | 50 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 50 °C | dry | 2 mm | UL746B | ||
Relative temperature index, mechanical strength | 50 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 50 °C | dry | 2 mm | UL746B | ||
Vicat softening temperature | 90 °C Show Supplier Material materials with Vicat softening temperature of 90 °C | dry | ISO 306 | 50°C/h 50N |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 600 V Show Supplier Material materials with Comparative tracking index of 600 V | dry | IEC 60112 | |
Dielectric constant | 5.2 [-] Show Supplier Material materials with Dielectric constant of 5.2 [-] | dry | IEC 62631-2-1 | 100Hz |
Dielectric strength | 20 kV/mm Show Supplier Material materials with Dielectric strength of 20 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 0.02 [-] Show Supplier Material materials with Dissipation factor of 0.02 [-] | dry | IEC 62631-2-1 | 100Hz |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt mass-flow rate | 230 °C | 14.4 g/10min Show Supplier Material materials with Melt mass-flow rate of 14.4 g/10min | dry | ISO 1133 | |
Melt volume-flow rate | 230 °C | 15 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 15 cm³/10min | dry | ISO 1133 | |
Shrinkage | 1.35 % Show Supplier Material materials with Shrinkage of 1.35 % | dry | Sim. to ISO 294-4 | Parallel | |
1.35 % Show Supplier Material materials with Shrinkage of 1.35 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available |