General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.61 g/cm³ Show Supplier Material materials with Density of 1.61 g/cm³ | dry | ISO 1183 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 14 GPa Show Supplier Material materials with Elastic modulus of 14 GPa | dry | ISO 527-1/-2 | |
Elongation | 1.1 % Show Supplier Material materials with Elongation of 1.1 % | dry | ISO 527-1/-2 | |
Impact strength, Charpy notched | 23 °C | 4.4 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 4.4 kJ/m² | dry | ISO 179/1eA |
Tensile strength | 90 MPa Show Supplier Material materials with Tensile strength of 90 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Thermal conductivity | 1.1 W/(m·K) Show Supplier Material materials with Thermal conductivity of 1.1 W/(m·K) | dry | ASTM E1461 | through plane |
5.1 W/(m·K) Show Supplier Material materials with Thermal conductivity of 5.1 W/(m·K) | dry | ASTM E1461 | in plane |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Dielectric constant | 4.22 [-] Show Supplier Material materials with Dielectric constant of 4.22 [-] | dry | IEC 60250 | 1GHz |
4.24 [-] Show Supplier Material materials with Dielectric constant of 4.24 [-] | dry | IEC 60250 | 5GHz | |
Dissipation factor | 70 [-] Show Supplier Material materials with Dissipation factor of 70 [-] | dry | IEC 60250 | 5GHz |
80 [-] Show Supplier Material materials with Dissipation factor of 80 [-] | dry | IEC 60250 | 1GHz | |
Surface resistivity | 6e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 6e+10 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 7e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 7e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Spiral flow length | 140 | dry | - | 1.0 mm 1000 bar |
Technological properties
Property | ||
---|---|---|
Fillers | 10% Glass Fiber |