Arnite® Care T1U

Want to keep this datasheet? Save it now in your required format

Description

Arnite® (PBT, PET and blends) are high-performance engineering plastics that combine high strength and rigidity with excellent processing characteristics. As a result, Arnite® A (PET)  and Arnite® T (PBT) are well suited for a broad range of automotive, electrical & electronic and consumer goods applications.
A wide portfolio of Arnite® is available including unreinforced, reinforced and flame retardant grades.

Datasheet URL:

Arnite® Care T1U

This material data has been provided by DSM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.33 g/cm³

Show Supplier Material materials with Density of 1.33 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.18 %

Show Supplier Material materials with Moisture absorption of 0.18 %

Sim. to ISO 62

Water absorption

23.0 °C

0.45 %

Show Supplier Material materials with Water absorption of 0.45 %

Sim. to ISO 62

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.7 GPa

Show Supplier Material materials with Elastic modulus of 2.7 GPa

ISO 527-1/-2

Elongation

23.0 °C

20 %

Show Supplier Material materials with Elongation of 20 %

ISO 527-1/-2

Elongation at yield

23.0 °C

3.5 - 55 %

Show Supplier Material materials with Elongation at yield of 3.5 - 55 %

ISO 527-1/-2

Impact strength, Charpy notched

-30.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

ISO 179/1eA

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

ISO 179/1eU

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

9E-7 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 9E-7 1/K

ISO 11359-1/-2, Parallel

Coefficient of thermal expansion, transverse

23.0 °C

9E-7 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 9E-7 1/K

ISO 11359-1/-2, Normal

Heat deflection temperature, 0.45 MPa

165 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 165 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

55 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 55 °C

ISO 75-1/-2

Melting point

225 °C

Show Supplier Material materials with Melting point of 225 °C

ISO 11357-1/-3, (10°C/min)

Thermal diffusivity

23.0 °C

4.65E-8 mm²/s

Show Supplier Material materials with Thermal diffusivity of 4.65E-8 mm²/s

-, Eff.

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Supplier Material materials with Comparative tracking index of 600 V

IEC 60112

Dielectric constant

23.0 °C

3.5 [-]

Show Supplier Material materials with Dielectric constant of 3.5 [-]

IEC 62631-2-1, 100Hz

Dielectric strength

23.0 °C

27 kV/mm

Show Supplier Material materials with Dielectric strength of 27 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

20 [-]

Show Supplier Material materials with Dissipation factor, 100Hz of 20 [-]

IEC 62631-2-1, 100Hz

Dissipation factor, 1MHz

23.0 °C

200 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 200 [-]

IEC 62631-2-1, 1 MHz

Volume resistivity

23.0 °C

1.00E+13 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+13 Ω·cm

IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Density of melt

1040 g/cm³

Show Supplier Material materials with Density of melt of 1040 g/cm³

-, Of melt

Melt mass-flow rate

27 g/10min

Show Supplier Material materials with Melt mass-flow rate of 27 g/10min

ISO 1133, 2.16 Kg

Melt volume-flow rate

24 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 24 cm³/10min

ISO 1133, 250 C, 2.16 Kg

Shrinkage

23.0 °C

2 %

Show Supplier Material materials with Shrinkage of 2 %

Sim. to ISO 294-4, Parallel

Shrinkage, transverse

23.0 °C

2 %

Show Supplier Material materials with Shrinkage, transverse of 2 %

Sim. to ISO 294-4, Normal

Specific heat capacity melt

2260 J/(kg·K)

Show Supplier Material materials with Specific heat capacity melt of 2260 J/(kg·K)

-, Of melt

Thermal conductivity of melt

0.11 W/(m·K)

Show Supplier Material materials with Thermal conductivity of melt of 0.11 W/(m·K)

-, Of melt

Technological properties

Property