Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Bio-based content | 22 % Show Supplier Material materials with Bio-based content of 22 % | dry | ASTM D6866-12 Method B | |
Density | 1.23 g/cm³ Show Supplier Material materials with Density of 1.23 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.01 % Show Supplier Material materials with Moisture absorption of 0.01 % | dry | Sim. to ISO 62 | |
Water absorption | 0.15 % Show Supplier Material materials with Water absorption of 0.15 % | dry | ISO 62 | at 23°C after 24h |
Mechanical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Elastic modulus | 0.34 GPa Show Supplier Material materials with Elastic modulus of 0.34 GPa | dry | ISO 527-1/-2 | |
Elongation | 105 % Show Supplier Material materials with Elongation of 105 % | dry | ISO 527-1/-2 | |
640 % Show Supplier Material materials with Elongation of 640 % | dry | ISO 527-1/-2 | ||
Flexural modulus | 0.35 GPa Show Supplier Material materials with Flexural modulus of 0.35 GPa | dry | ISO 178 | |
Hardness, Shore D | 65 [-] Show Supplier Material materials with Hardness, Shore D of 65 [-] | dry | ISO 868 | 3s |
Tear strength | 169 kN/m Show Supplier Material materials with Tear strength of 169 kN/m | dry | ISO 34-1; Method B | |
190 kN/m Show Supplier Material materials with Tear strength of 190 kN/m | dry | ISO 34-1; Method B | ||
Tensile strength | 27 MPa Show Supplier Material materials with Tensile strength of 27 MPa | dry | ISO 527-1/-2 | |
49 MPa Show Supplier Material materials with Tensile strength of 49 MPa | dry | ISO 527-1/-2 | Normal |
Thermal
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Glass transition temperature | -2 °C Show Supplier Material materials with Glass transition temperature of -2 °C | dry | ISO 11357-1/-2 | 10°C/min |
Melting point | 210 °C Show Supplier Material materials with Melting point of 210 °C | dry | ISO 11357-1/-3 | 10°C/min |
Vicat softening temperature | 99 °C Show Supplier Material materials with Vicat softening temperature of 99 °C | dry | ISO 306 | 50°C/h 50N |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dielectric strength | 20 kV/mm Show Supplier Material materials with Dielectric strength of 20 kV/mm | dry | IEC 60243-1 |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt volume-flow rate | 230 °C | 5 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 5 cm³/10min | dry | ISO 1133 | |
Shrinkage | 1.5 % Show Supplier Material materials with Shrinkage of 1.5 % | dry | ISO 294-4 | Parallel | |
1.5 % Show Supplier Material materials with Shrinkage of 1.5 % | dry | Sim. to ISO 294-4 | Parallel | ||
1.75 % Show Supplier Material materials with Shrinkage of 1.75 % | dry | ISO 294-4 | Normal | ||
1.75 % Show Supplier Material materials with Shrinkage of 1.75 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Application areas | Cooking Bag, Bio-based panliners, Snowboard Cover Laminates, Smokable Sausage Casings | |
Certifications | Food Contact |