General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.85 g/cm³ Show Supplier Material materials with Density of 1.85 g/cm³ | dry | ISO 1183 | |
Water absorption | 0.04 % Show Supplier Material materials with Water absorption of 0.04 % | dry | ISO 62 | at 23°C after 24h |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 23 GPa Show Supplier Material materials with Elastic modulus of 23 GPa | dry | ISO 527-1/-2 |
22 GPa Show Supplier Material materials with Elastic modulus of 22 GPa | dry | ISO 527-1/-2 | ||
120 °C | 12.2 GPa Show Supplier Material materials with Elastic modulus of 12.2 GPa | dry | ISO 527-1/-2 | |
160 °C | 9.9 GPa Show Supplier Material materials with Elastic modulus of 9.9 GPa | dry | ISO 527-1/-2 | |
180 °C | 9.2 GPa Show Supplier Material materials with Elastic modulus of 9.2 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 0.75 % Show Supplier Material materials with Elongation of 0.75 % | dry | ISO 527-1/-2 |
0.7 % Show Supplier Material materials with Elongation of 0.7 % | dry | ISO 527-1/-2 | ||
120 °C | 1.2 % Show Supplier Material materials with Elongation of 1.2 % | dry | ISO 527-1/-2 | |
160 °C | 1.5 % Show Supplier Material materials with Elongation of 1.5 % | dry | ISO 527-1/-2 | |
180 °C | 1.3 % Show Supplier Material materials with Elongation of 1.3 % | dry | ISO 527-1/-2 | |
Flexural modulus | 23.2 GPa Show Supplier Material materials with Flexural modulus of 23.2 GPa | dry | ISO 178 | |
120 °C | 13.8 GPa Show Supplier Material materials with Flexural modulus of 13.8 GPa | dry | ISO 178 | |
160 °C | 11 GPa Show Supplier Material materials with Flexural modulus of 11 GPa | dry | ISO 178 | |
180 °C | 10.1 GPa Show Supplier Material materials with Flexural modulus of 10.1 GPa | dry | ISO 178 | |
Flexural yield strength | 215 MPa Show Supplier Material materials with Flexural yield strength of 215 MPa | dry | ISO 178 | |
120 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |
160 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
180 °C | 95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | |
Hardness, Rockwell M | 100 [-] Show Supplier Material materials with Hardness, Rockwell M of 100 [-] | dry | ISO 2039-2 | |
Hardness, Rockwell R | 120 [-] Show Supplier Material materials with Hardness, Rockwell R of 120 [-] | dry | ISO 2039-2 | |
Impact strength, Charpy notched | -30 °C | 9 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m² | dry | ISO 179/1eA |
23 °C | 9 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 16 kJ/m² | dry | ISO 179/1eU |
23 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 16 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | -40 °C | 138 MPa Show Supplier Material materials with Tensile strength of 138 MPa | dry | ISO 527-1/-2 |
120 MPa Show Supplier Material materials with Tensile strength of 120 MPa | dry | ISO 527-1/-2 | ||
120 °C | 78.5 MPa Show Supplier Material materials with Tensile strength of 78.5 MPa | dry | ISO 527-1/-2 | |
160 °C | 63 MPa Show Supplier Material materials with Tensile strength of 63 MPa | dry | ISO 527-1/-2 | |
180 °C | 55.0 MPa Show Supplier Material materials with Tensile strength of 55.0 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Thickness | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 1.1e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.1e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
1.2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.2e-07 1/K | dry | ISO 11359-1/-2 | parallel, above Tg | |||
3e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
7.2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 7.2e-07 1/K | dry | ISO 11359-1/-2 | normal, above Tg | |||
Glass transition temperature | 90 °C Show Supplier Material materials with Glass transition temperature of 90 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Heat deflection temperature | 265 °C Show Supplier Material materials with Heat deflection temperature of 265 °C | dry | ISO 75-1/-2 | 2 MPa | ||
Melting point | 280 °C Show Supplier Material materials with Melting point of 280 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | dry | UL746B | 0.4 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.4 mm | ||
Thermal conductivity | 1.2 W/(m·K) Show Supplier Material materials with Thermal conductivity of 1.2 W/(m·K) | dry | ASTM E1461 | through plane | ||
2.2 W/(m·K) Show Supplier Material materials with Thermal conductivity of 2.2 W/(m·K) | dry | ASTM E1461 | in plane |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Comparative tracking index | 225 V Show Supplier Material materials with Comparative tracking index of 225 V | dry | IEC 60112 |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 60% Glass Fiber and Mineral Powder |