General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.41 g/cm³ Show Supplier Material materials with Density of 1.41 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Water absorption | 0.3 % Show Supplier Material materials with Water absorption of 0.3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 6.8 GPa Show Supplier Material materials with Elastic modulus of 6.8 GPa | dry | ISO 527-1/-2 |
6 GPa Show Supplier Material materials with Elastic modulus of 6 GPa | dry | ISO 527-1/-2 | ||
100 °C | 2.5 GPa Show Supplier Material materials with Elastic modulus of 2.5 GPa | dry | ISO 527-1/-2 | |
120 °C | 2.3 GPa Show Supplier Material materials with Elastic modulus of 2.3 GPa | dry | ISO 527-1/-2 | |
160 °C | 1.8 GPa Show Supplier Material materials with Elastic modulus of 1.8 GPa | dry | ISO 527-1/-2 | |
180 °C | 1.6 GPa Show Supplier Material materials with Elastic modulus of 1.6 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 2.3 % Show Supplier Material materials with Elongation of 2.3 % | dry | ISO 527-1/-2 |
3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | ||
120 °C | 7 % Show Supplier Material materials with Elongation of 7 % | dry | ISO 527-1/-2 | |
160 °C | 7 % Show Supplier Material materials with Elongation of 7 % | dry | ISO 527-1/-2 | |
180 °C | 7 % Show Supplier Material materials with Elongation of 7 % | dry | ISO 527-1/-2 | |
Flexural modulus | 5.6 GPa Show Supplier Material materials with Flexural modulus of 5.6 GPa | dry | ISO 178 | |
120 °C | 2.3 GPa Show Supplier Material materials with Flexural modulus of 2.3 GPa | dry | ISO 178 | |
160 °C | 2 GPa Show Supplier Material materials with Flexural modulus of 2 GPa | dry | ISO 178 | |
Flexural yield strength | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |
120 °C | 70 MPa Show Supplier Material materials with Flexural yield strength of 70 MPa | dry | ISO 178 | |
160 °C | 55.0 MPa Show Supplier Material materials with Flexural yield strength of 55.0 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 6 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 6 kJ/m² | dry | ISO 179/1eA |
23 °C | 6 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 6 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 32 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 32 kJ/m² | dry | ISO 179/1eU |
23 °C | 34 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 34 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | -40 °C | 125 MPa Show Supplier Material materials with Tensile strength of 125 MPa | dry | ISO 527-1/-2 |
115 MPa Show Supplier Material materials with Tensile strength of 115 MPa | dry | ISO 527-1/-2 | ||
100 °C | 55.0 MPa Show Supplier Material materials with Tensile strength of 55.0 MPa | dry | ISO 527-1/-2 | |
120 °C | 50 MPa Show Supplier Material materials with Tensile strength of 50 MPa | dry | ISO 527-1/-2 | |
160 °C | 40 MPa Show Supplier Material materials with Tensile strength of 40 MPa | dry | ISO 527-1/-2 | |
180 °C | 33 MPa Show Supplier Material materials with Tensile strength of 33 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
8e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Heat deflection temperature | 195 °C Show Supplier Material materials with Heat deflection temperature of 195 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 225 °C Show Supplier Material materials with Melting point of 225 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 400 V Show Supplier Material materials with Comparative tracking index of 400 V | dry | IEC 60112 | |
Dielectric constant | 3.4 [-] Show Supplier Material materials with Dielectric constant of 3.4 [-] | dry | IEC 62631-2-1 | 1MHz |
3.6 [-] Show Supplier Material materials with Dielectric constant of 3.6 [-] | dry | IEC 62631-2-1 | 100Hz | |
Dissipation factor | 20 [-] Show Supplier Material materials with Dissipation factor of 20 [-] | dry | IEC 62631-2-1 | 100Hz |
180 [-] Show Supplier Material materials with Dissipation factor of 180 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt volume-flow rate | 250 °C | 27 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 27 cm³/10min | dry | ISO 1133 | |
Shrinkage | 0.6 % Show Supplier Material materials with Shrinkage of 0.6 % | dry | Sim. to ISO 294-4 | Parallel | |
1.4 % Show Supplier Material materials with Shrinkage of 1.4 % | dry | Sim. to ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Application areas | Actuator Covers, Automotive Connectors (3) | |
Fillers | 15% Glass Fiber |