Description

Pt-10%Rh DPH-A is an oxide dispersion hardened alloy from the Heraeus DPH class of materials with very high creep strength at temperatures up to 1700°C.

This material data has been provided by Heraeus.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValue

Density

23.0 °C

19.87 g/cm³

Show Supplier Material materials with Density of 19.87 g/cm³

Mechanical

PropertyTemperatureValueComment

Creep strength

1200.0 °C

7.6 MPa

Show Supplier Material materials with Creep strength of 7.6 MPa

10,000 h (extrapolated data)

1400.0 °C

6.8 MPa

Show Supplier Material materials with Creep strength of 6.8 MPa

10,000 h (extrapolated data)

1600.0 °C

4.6 MPa

Show Supplier Material materials with Creep strength of 4.6 MPa

10,000 h (extrapolated data)

Elastic modulus

1200.0 °C

142.2 GPa

Show Supplier Material materials with Elastic modulus of 142.2 GPa

Elongation

1200.0 °C

28 %

Show Supplier Material materials with Elongation of 28 %

1400.0 °C

32 %

Show Supplier Material materials with Elongation of 32 %

1600.0 °C

56 %

Show Supplier Material materials with Elongation of 56 %

Unlock all property charts

Hardness, Vickers

23.0 °C

130 [-]

Show Supplier Material materials with Hardness, Vickers of 130 [-]

Norton Exponent

1200.0 °C

6.7 [-]

Show Supplier Material materials with Norton Exponent of 6.7 [-]

1400.0 °C

11.6 [-]

Show Supplier Material materials with Norton Exponent of 11.6 [-]

1600.0 °C

11 [-]

Show Supplier Material materials with Norton Exponent of 11 [-]

Unlock all property charts

Tensile strength

1200.0 °C

85 MPa

Show Supplier Material materials with Tensile strength of 85 MPa

1400.0 °C

52 MPa

Show Supplier Material materials with Tensile strength of 52 MPa

1600.0 °C

31 MPa

Show Supplier Material materials with Tensile strength of 31 MPa

Unlock all property charts

Yield strength Rp0.2

1200.0 °C

57 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 57 MPa

1400.0 °C

40 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 40 MPa

1600.0 °C

27 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 27 MPa

Unlock all property charts

Thermal

PropertyTemperatureValue

Melting point

1840 - 1870 °C

Show Supplier Material materials with Melting point of 1840 - 1870 °C

Thermal conductivity

20.0 °C

40.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 40.3 W/(m·K)

1200.0 °C

66.7 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 66.7 W/(m·K)

1400.0 °C

69.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 69.5 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.5E-7 Ω·m

Show Supplier Material materials with Electrical resistivity of 1.5E-7 Ω·m

1156.0 °C

5.5E-7 Ω·m

Show Supplier Material materials with Electrical resistivity of 5.5E-7 Ω·m

1400.0 °C

6.1E-7 Ω·m

Show Supplier Material materials with Electrical resistivity of 6.1E-7 Ω·m