VYPET™ VNT-930

Alternative and trade names
PET-GF30
Want to keep this datasheet? Save it now in your required format

Description

Polyethylene Terephthalate (PET) with 30% Glass Fiber Reinforced. Contains a minimum of 58% Post-consumer resin

This material data has been provided by Lavergne.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyValue

Recycled Content

58 %

Show Supplier Material materials with Recycled Content of 58 %

Mechanical

PropertyTemperatureValueComment

Flexural modulus

23.0 °C

9.4 GPa

Show Supplier Material materials with Flexural modulus of 9.4 GPa

ASTM D790

Flexural strength

23.0 °C

205 MPa

Show Supplier Material materials with Flexural strength of 205 MPa

ASTM D790

Impact strength, Izod notched, ASTM

23.0 °C

100 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 100 J/m

ASTM D256

Tensile strength

23.0 °C

132 MPa

Show Supplier Material materials with Tensile strength of 132 MPa

ASTM D638

Thermal

PropertyTemperatureValueComment

Ash content

23.0 °C

30 %

Show Supplier Material materials with Ash content of 30 %

ASTM D5630

Heat deflection temperature, 1.80 MPa

220 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 220 °C

ASTM D648

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.4 %

Show Supplier Material materials with Shrinkage of 0.4 %

ASTM D955

Shrinkage, transverse

23.0 °C

0.8 %

Show Supplier Material materials with Shrinkage, transverse of 0.8 %

ASTM D955

Technological properties

Property
Application areas

Sunroof rails,Structural applications (e.g. grill retainers and lamp holders).

Certifications

RoHS,RECH,ULE Environmental Claims Validation

Color

Black

Fillers

30% Glass Fiber

Processing methods

  • Drying to Dew Point:-18°C or lower
  • Feed zone: 260-270°C
  • Middle zone: 265-290°C
  • Front zone: 270-295°C
  • Nozzle: 280-300°C
  • Melt temperature: 275-290°C
  • Mold temperature (thick wall parts): 95-120°C
  • Mold temperature (thin wall parts): 95-120°C
  • Injection Pressure: Medium
  • Injection Speed: Medium
  • Back Pressure: Low
  • Screw Speed: Medium