General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastic modulus of 60.0 - 70.0 GPa | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | ||
Elongation | 20.0 °C | 22.0 % Show Material materials with Elongation of 22.0 % | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | A10 |
20.0 °C | 25.0 % Show Material materials with Elongation of 25.0 % | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | ||
Hardness, Brinell | 18.0 [-] Show Material materials with Hardness, Brinell of 18.0 [-] | F | EN 573-3, EN 485 | |||
19.0 [-] Show Material materials with Hardness, Brinell of 19.0 [-] | F | EN 573-3, EN 570 | ||||
20.0 °C | 18.0 [-] Show Material materials with Hardness, Brinell of 18.0 [-] | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 25.0 GPa Show Material materials with Shear modulus of 25.0 GPa | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | |
Tensile strength | 60.0 MPa Show Material materials with Tensile strength of 60.0 MPa | F | EN 573-3, EN 485 | |||
80.0 - 110.0 MPa Show Material materials with Tensile strength of 80.0 - 110.0 MPa | F | EN 573-3, EN 1715-3, EN 1715-4 | ||||
20.0 °C | 55.0 MPa Show Material materials with Tensile strength of 55.0 MPa | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile | ||
20.0 °C | 60.0 MPa Show Material materials with Tensile strength of 60.0 MPa | F | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | |
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | ||
Melting point | 659.0 °C Show Material materials with Melting point of 659.0 °C | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | ||
Specific heat capacity | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Specific heat capacity of 921.0 J/(kg·K) | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube |
Thermal conductivity | 225 W/(m·K) Show Material materials with Thermal conductivity of 225 W/(m·K) | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | ||
20.0 °C | 215.0 W/(m·K) Show Material materials with Thermal conductivity of 215.0 W/(m·K) | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 34500000.0 - 35000000.0 S/m Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | ||
20.0 °C | 36400000.0 - 37000000.0 S/m Show Material materials with Electrical conductivity of 36400000.0 - 37000000.0 S/m | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube | |
Electrical resistivity | 2.86e-08 - 2.9e-08 Ω·m Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.8 % Show Material materials with Aluminium of 99.8 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | |
Copper | 0.03 % Show Material materials with Copper of 0.03 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Gallium | 0.03 % Show Material materials with Gallium of 0.03 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Iron | 0.15 % Show Material materials with Iron of 0.15 % | F | DIN 1712-3, EN 573-3, EN 573-4 | Profile, Rod, Tube |
0.15 % Show Material materials with Iron of 0.15 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 570 | ||
Magnesium | 0.02 % Show Material materials with Magnesium of 0.02 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Manganese | 0.02 % Show Material materials with Manganese of 0.02 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Silicon | 0.15 % Show Material materials with Silicon of 0.15 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Titanium | 0.02 % Show Material materials with Titanium of 0.02 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Zinc | 0.06 % Show Material materials with Zinc of 0.06 % | F | DIN 1712-3, EN 573-3, EN 573-4, EN 1715-3, EN 1715-4, EN 485, EN 570 | Profile, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: very good, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |