General
Property | Value | Comment |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | Typical for Wrought 6000 Series Aluminium |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Elongation | -75.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T5 | DIN 1725-1 | Seamless Tube | Transverse |
-75.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
50.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
50.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
100.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.0 - 26.5 GPa Show Material materials with Shear modulus of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Tensile strength | -75.0 °C | 275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T5 | DIN 1725-1 | Seamless Tube | |
-75.0 °C | 275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
-75.0 °C | 310.0 MPa Show Material materials with Tensile strength of 310.0 MPa | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
-75.0 °C | 310.0 MPa Show Material materials with Tensile strength of 310.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
20.0 °C | 225.0 MPa Show Material materials with Tensile strength of 225.0 MPa | T5 | DIN 1725-1 | Tube | ||
20.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T5 | DIN 1725-1 | Rod, Seamless Tube | ||
20.0 °C | 275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T5 | DIN 1725-1 | Seamless Tube | ||
20.0 °C | 275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
20.0 °C | 310.0 MPa Show Material materials with Tensile strength of 310.0 MPa | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | ||
20.0 °C | 310.0 MPa Show Material materials with Tensile strength of 310.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
20.0 °C | 390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T5 | DIN 1725-1 | Rod | ||
50.0 °C | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | T5 | DIN 1725-1 | Rod | ||
50.0 °C | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | T5 | DIN 1725-1 | |||
50.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T5 | DIN 1725-1 | Rod, Seamless Tube | ||
50.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
50.0 °C | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | T5 | DIN 1725-1 | Rod | ||
50.0 °C | 280.0 MPa Show Material materials with Tensile strength of 280.0 MPa | T5 | DIN 1725-1 | Tube, Seamless Tube | ||
50.0 °C | 280.0 MPa Show Material materials with Tensile strength of 280.0 MPa | T5 | DIN 1725-1 | Seamless Tube | Transverse | |
50.0 °C | 290.0 MPa Show Material materials with Tensile strength of 290.0 MPa | T5 | DIN 1725-1 | Rod, Tube | ||
50.0 °C | 300.0 MPa Show Material materials with Tensile strength of 300.0 MPa | T5 | DIN 1725-1 | Rod, Tube | ||
100.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | T5 | DIN 1725-1 | Rod | ||
100.0 °C | 210.0 MPa Show Material materials with Tensile strength of 210.0 MPa | T5 | DIN 1725-1 | Rod | ||
100.0 °C | 250.0 MPa Show Material materials with Tensile strength of 250.0 MPa | T5 | DIN 1725-1 | Rod, Seamless Tube | ||
100.0 °C | 280.0 MPa Show Material materials with Tensile strength of 280.0 MPa | T5 | DIN 1725-1 | Tube, Seamless Tube | ||
100.0 °C | 290.0 MPa Show Material materials with Tensile strength of 290.0 MPa | T5 | DIN 1725-1 | Rod, Tube | ||
100.0 °C | 335.0 MPa Show Material materials with Tensile strength of 335.0 MPa | T5 | DIN 1725-1 | Rod |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Melting point | 555.0 - 655.0 °C Show Material materials with Melting point of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Specific heat capacity | 887.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Thermal conductivity | 170.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 21000000.0 - 34000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
Electrical resistivity | 2.9e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 - 0.25 % Show Material materials with Chromium of 0.1 - 0.25 % | T5 | DIN 1725-1 | Rod, Tube |
0.1 - 0.2 % Show Material materials with Chromium of 0.1 - 0.2 % | T5 | DIN 1725-1 | Seamless Tube | |
0.2 % Show Material materials with Chromium of 0.2 % | T5 | DIN 1725-1 | Seamless Tube | |
0.25 % Show Material materials with Chromium of 0.25 % | T5 | DIN 1725-1 | Rod | |
Copper | 0.05 Show Material materials with Copper of 0.05 | T5 | DIN 1725-1 | Tube |
0.1 Show Material materials with Copper of 0.1 | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube | |
Iron | 0.4 Show Material materials with Iron of 0.4 | T5 | DIN 1725-1 | Seamless Tube, Tube |
0.5 Show Material materials with Iron of 0.5 | T5 | DIN 1725-1 | Rod, Tube | |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube |
1.2 % Show Material materials with Magnesium of 1.2 % | T5 | DIN 1725-1 | Seamless Tube | |
Manganese | 0.4 - 1.0 % Show Material materials with Manganese of 0.4 - 1.0 % | T5 | DIN 1725-1 | Rod, Tube |
0.4 - 0.8 % Show Material materials with Manganese of 0.4 - 0.8 % | T5 | DIN 1725-1 | Seamless Tube | |
0.8 % Show Material materials with Manganese of 0.8 % | T5 | DIN 1725-1 | Seamless Tube | |
Silicon | 0.7 - 1.3 % Show Material materials with Silicon of 0.7 - 1.3 % | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube |
0.75 - 1.3 % Show Material materials with Silicon of 0.75 - 1.3 % | T5 | DIN 1725-1 | Tube | |
1.3 % Show Material materials with Silicon of 1.3 % | T5 | DIN 1725-1 | Seamless Tube | |
Titanium | 0.1 Show Material materials with Titanium of 0.1 | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube |
Zinc | 0.2 Show Material materials with Zinc of 0.2 | T5 | DIN 1725-1 | Rod, Tube, Seamless Tube |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |