General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 MPa | T5 | EN 573-3, EN 755 | |||
Elastic modulus | 69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | T5 | EN 573-3, EN 755 | |||
20.0 °C | 67.0 GPa Show Material materials with Elastic modulus of 67.0 GPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
Elongation | 6.0 % Show Material materials with Elongation of 6.0 % | T5 | EN 573-3, EN 755 | A50 | ||
8.0 % Show Material materials with Elongation of 8.0 % | T5 | EN 573-3, EN 755 | A100 | |||
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T5 | DIN 1725-1 | Seamless Tube | ||
50.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T5 | DIN 1725-1 | Seamless Tube | ||
100.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T5 | DIN 1725-1 | Seamless Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | T5 | EN 573-3, EN 755 | |||
20.0 °C | 25.0 GPa Show Material materials with Shear modulus of 25.0 GPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
Tensile strength | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | T5 | EN 573-3, EN 755 | |||
160.0 MPa Show Material materials with Tensile strength of 160.0 MPa | T5 | EN 573-3, EN 755 | ||||
20.0 °C | 215.0 MPa Show Material materials with Tensile strength of 215.0 MPa | T5 | DIN 1725-1 | Seamless Tube | ||
20.0 °C | 246.0 MPa Show Material materials with Tensile strength of 246.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
50.0 °C | 210.0 MPa Show Material materials with Tensile strength of 210.0 MPa | T5 | DIN 1725-1 | Seamless Tube | ||
100.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | T5 | DIN 1725-1 | Seamless Tube | ||
100.0 °C | 232.0 MPa Show Material materials with Tensile strength of 232.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
150.0 °C | 152.0 MPa Show Material materials with Tensile strength of 152.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
200.0 °C | 63.0 MPa Show Material materials with Tensile strength of 63.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
250.0 °C | 35.0 MPa Show Material materials with Tensile strength of 35.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
320.0 °C | 18.0 MPa Show Material materials with Tensile strength of 18.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |||
370.0 °C | 14.0 MPa Show Material materials with Tensile strength of 14.0 MPa | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 |
Thermal
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.18e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K | T5 | EN 573-3, EN 755 |
20 °C | 2.18e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K | T5 | EN 573-3, EN 755 | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T5 | EN 573-3, EN 755 | |
20 °C | 2.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K | T5 | EN 573-3, EN 755 | |
20 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | T5 | EN 573-3, EN 755 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T5 | EN 573-3, EN 755 | |
200 °C | 2.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K | T5 | EN 573-3, EN 755 | |
300 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | T5 | EN 573-3, EN 755 | |
Melting point | 585.0 - 650.0 °C Show Material materials with Melting point of 585.0 - 650.0 °C | T5 | EN 573-3, EN 755 | |
Specific heat capacity | 898.0 J/(kg·K) Show Material materials with Specific heat capacity of 898.0 J/(kg·K) | T5 | EN 573-3, EN 755 | |
Thermal conductivity | 200.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 200.0 - 220.0 W/(m·K) | T5 | EN 573-3, EN 755 | |
20.0 °C | 220.0 W/(m·K) Show Material materials with Thermal conductivity of 220.0 W/(m·K) | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 |
Electrical
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Electrical conductivity | 34000000.0 - 38000000.0 S/m Show Material materials with Electrical conductivity of 34000000.0 - 38000000.0 S/m | T5 | EN 573-3, EN 755 | |
20.0 °C | 30000000.0 - 32000000.0 S/m Show Material materials with Electrical conductivity of 30000000.0 - 32000000.0 S/m | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | |
Electrical resistivity | 2.63e-08 - 2.94e-08 Ω·m Show Material materials with Electrical resistivity of 2.63e-08 - 2.94e-08 Ω·m | T5 | EN 573-3, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.05 % Show Material materials with Chromium of 0.05 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Iron | 0.1 - 0.3 % Show Material materials with Iron of 0.1 - 0.3 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Magnesium | 0.35 - 0.6 % Show Material materials with Magnesium of 0.35 - 0.6 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Silicon | 0.3 - 0.6 % Show Material materials with Silicon of 0.3 - 0.6 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Zinc | 0.15 % Show Material materials with Zinc of 0.15 % | T5 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 755 | Seamless Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: EQ: sehr gut, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) - / good (O) |