EN 573-3 Grade AW-1050A H111

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

0.2 mm

Coil, Sheet, Strip

3 mm

Show Material materials with Thickness of 3 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

3 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-195.0 °C

78.4 GPa

Show Material materials with Elastic modulus of 78.4 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

-85.0 °C

73.5 GPa

Show Material materials with Elastic modulus of 73.5 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

-30.0 °C

71.4 GPa

Show Material materials with Elastic modulus of 71.4 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

100.0 °C

68.0 - 68.6 GPa

Show Material materials with Elastic modulus of 68.0 - 68.6 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

100.0 °C

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

150.0 °C

66.0 - 66.5 GPa

Show Material materials with Elastic modulus of 66.0 - 66.5 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

150.0 °C

66.5 GPa

Show Material materials with Elastic modulus of 66.5 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

250.0 °C

56.0 - 57.0 GPa

Show Material materials with Elastic modulus of 56.0 - 57.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

250.0 °C

56.0 GPa

Show Material materials with Elastic modulus of 56.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

Elongation

20 %

Show Material materials with Elongation of 20 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

A50

20.0 %

Show Material materials with Elongation of 20.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

22.0 %

Show Material materials with Elongation of 22.0 %

H111

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

23.0 %

Show Material materials with Elongation of 23.0 %

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

26.0 %

Show Material materials with Elongation of 26.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

H111

EN 573-3

Flat

A50

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

H111

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

H111

EN 573-3

Rod, Tube

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3

Rod, Tube

20.0 °C

26.0 %

Show Material materials with Elongation of 26.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

26.0 %

Show Material materials with Elongation of 26.0 %

H111

EN 573-3

Flat

A50

20.0 °C

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3

Flat

A50

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

Transverse

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Sheet, Strip

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Flat

A50

Hardness, Brinell

20.0 [-]

Show Material materials with Hardness, Brinell of 20.0 [-]

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

20.0 [-]

Show Material materials with Hardness, Brinell of 20.0 [-]

H111

EN 573-3

Flat, Rod, Tube

Hardness, HBW

20 [-]

Show Material materials with Hardness, HBW of 20 [-]

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

25.0 - 25.9 GPa

Show Material materials with Shear modulus of 25.0 - 25.9 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

25.9 - 26.5 GPa

Show Material materials with Shear modulus of 25.9 - 26.5 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

H111

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

65.0 MPa

Show Material materials with Tensile strength of 65.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 95.0 MPa

Show Material materials with Tensile strength of 60.0 - 95.0 MPa

H111

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

20.0 °C

65.0 - 95.0 MPa

Show Material materials with Tensile strength of 65.0 - 95.0 MPa

H111

EN 573-3

Flat

Transverse

20.0 °C

65.0 MPa

Show Material materials with Tensile strength of 65.0 MPa

H111

EN 573-3

Rod, Sheet, Strip, Tube

20.0 °C

65.0 - 95.0 MPa

Show Material materials with Tensile strength of 65.0 - 95.0 MPa

H111

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Coil, Sheet, Strip

Yield strength

-270 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

H111

EN 573-3

Rod, Sheet, Strip, Tube, Plate, Foil, Bar

RP1

-270.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

H111

EN 573-3

Rod, Sheet, Strip, Tube, Plate, Foil, Bar

RP1

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

H111

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

20 MPa

Show Material materials with Yield strength of 20 MPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

H111

EN 573-3

Flat

RP02 Transverse

20.0 °C

20.0 - 60.0 MPa

Show Material materials with Yield strength of 20.0 - 60.0 MPa

H111

EN 573-3

Rod, Tube

RP02

20.0 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

H111

EN 573-3

Rod, Tube, Flat

RP02

20.0 °C

20.0 - 55.0 MPa

Show Material materials with Yield strength of 20.0 - 55.0 MPa

H111

EN 573-3

Sheet, Strip, Plate, Foil, Bar, Rod, Tube

RP02

20.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

H111

EN 573-3

Rod, Sheet, Strip, Tube, Plate, Foil, Bar

RP1

20 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

H111

EN 573-3

Rod, Sheet, Strip, Tube, Plate, Foil, Bar

RP1

50.0 °C

29.0 MPa

Show Material materials with Yield strength of 29.0 MPa

H111

EN 573-3

RP1

100 °C

13.0 MPa

Show Material materials with Yield strength of 13.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP1

100.0 °C

27.0 MPa

Show Material materials with Yield strength of 27.0 MPa

H111

EN 573-3

RP1

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20-100°C

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Melting point

646.0 - 657.0 °C

Show Material materials with Melting point of 646.0 - 657.0 °C

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

210.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 229.0 W/(m·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

220.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 - 229.0 W/(m·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

229.0 W/(m·K)

Show Material materials with Thermal conductivity of 229.0 W/(m·K)

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 36000000.0 S/m

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34800000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34800000.0 - 36000000.0 S/m

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Electrical resistivity

2.78e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.94e-08 Ω·m

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

2.8e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 2.9e-08 Ω·m

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

20.0 °C

2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 Ω·m

H111

EN 573-3

Rod, Sheet, Flat, Strip, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

Boron

0.05

Show Material materials with Boron of 0.05

H111

EN 573-3

Flat

Chromium

0.01

Show Material materials with Chromium of 0.01

H111

EN 573-3

Flat

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.05 %

Show Material materials with Copper of 0.05 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Gallium

0.03

Show Material materials with Gallium of 0.03

H111

EN 573-3

Flat

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-3

Flat, Rod, Sheet, Strip, Tube

0.40 %

Show Material materials with Iron of 0.40 %

H111

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

0.4 %

Show Material materials with Iron of 0.4 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H111

EN 573-3

Flat

0.05 %

Show Material materials with Magnesium of 0.05 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.05 %

Show Material materials with Magnesium of 0.05 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

H111

EN 573-3

Flat

0.05 %

Show Material materials with Manganese of 0.05 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.05 %

Show Material materials with Manganese of 0.05 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Nickel

0.03

Show Material materials with Nickel of 0.03

H111

EN 573-3

Flat

Other

0.03 %

Show Material materials with Other of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

H111

EN 573-3

Flat

0.25 %

Show Material materials with Silicon of 0.25 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.25 %

Show Material materials with Silicon of 0.25 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H111

EN 573-3

Flat

0.05 %

Show Material materials with Titanium of 0.05 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.05 %

Show Material materials with Titanium of 0.05 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Vanadium

0.03

Show Material materials with Vanadium of 0.03

H111

EN 573-3

Flat

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H111

EN 573-3

Flat

0.07 %

Show Material materials with Zinc of 0.07 %

H111

EN 573-3, EN 485, EN 754, EN 755

Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar

0.07 %

Show Material materials with Zinc of 0.07 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Lithography; Cable Wrapping: Electric cable wrapping; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, rotor hub, stairs; Cosmetics: Cosmetics pieces; Automotive Trim: Interior Trim, Marque Badges; Components: Heat shields, General Transportation

Brazing

Excellent

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent