EN 573-3 Grade AW-1070A H111

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H111

EN 573-3

Flat

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Strip

3 mm

Show Material materials with Thickness of 3 mm

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H111

EN 573-3

Flat

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H111

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H111

EN 573-3

Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H111

EN 573-3

Flat

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H111

EN 573-3

Flat

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H111

EN 573-3

Flat

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H111

EN 573-3

Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Elongation

23 %

Show Material materials with Elongation of 23 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2, A50

23.0 %

Show Material materials with Elongation of 23.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A100

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

A50

40.0 %

Show Material materials with Elongation of 40.0 %

H111

EN 573-3

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

H111

EN 573-3

Flat

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

H111

EN 573-3

Flat

A50

20.0 °C

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

29.0 %

Show Material materials with Elongation of 29.0 %

H111

EN 573-3

Flat

A50

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

Transverse

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

20.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

H111

EN 573-3

Flat

A50

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Flat

A50 Transverse

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

H111

EN 573-3

Flat

A50

20.0 °C

40.0 %

Show Material materials with Elongation of 40.0 %

H111

EN 573-3

Flat

Hardness, Brinell

18.0 [-]

Show Material materials with Hardness, Brinell of 18.0 [-]

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

18.0 [-]

Show Material materials with Hardness, Brinell of 18.0 [-]

H111

EN 573-3

Flat

Hardness, HBW

18 [-]

Show Material materials with Hardness, HBW of 18 [-]

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H111

EN 573-3

Flat

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

60.0 - 90.0 MPa

Show Material materials with Tensile strength of 60.0 - 90.0 MPa

H111

EN 573-3

Flat

Transverse

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

H111

EN 573-3

Flat

20.0 °C

60.0 - 90.0 MPa

Show Material materials with Tensile strength of 60.0 - 90.0 MPa

H111

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

according to EN 485-2

Yield strength

-270 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

RP1

-270.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

RP1

15.0 MPa

Show Material materials with Yield strength of 15.0 MPa

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

RP02

15 MPa

Show Material materials with Yield strength of 15 MPa

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

50.0 MPa

Show Material materials with Yield strength of 50.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Tube, Bar

RP02

20.0 °C

15.0 MPa

Show Material materials with Yield strength of 15.0 MPa

H111

EN 573-3

Flat

RP02 Transverse

20.0 °C

15.0 MPa

Show Material materials with Yield strength of 15.0 MPa

H111

EN 573-3

Flat

RP02

20.0 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

RP1

20 °C

25.0 MPa

Show Material materials with Yield strength of 25.0 MPa

H111

EN 573-3

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

RP1

20.0 °C

50.0 MPa

Show Material materials with Yield strength of 50.0 MPa

H111

EN 573-3

Flat

RP02

50.0 °C

23.0 MPa

Show Material materials with Yield strength of 23.0 MPa

H111

EN 573-3

RP1

100 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Tube, Bar

RP1

100.0 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

H111

EN 573-3

Strip, Sheet, Plate, Wire, Tube, Bar

RP1

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20-100°C

Melting point

659.0 °C

Show Material materials with Melting point of 659.0 °C

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H111

EN 573-3

Flat

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

225 W/(m·K)

Show Material materials with Thermal conductivity of 225 W/(m·K)

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

215.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 W/(m·K)

H111

EN 573-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34500000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

20.0 °C

35800000.0 - 36800000.0 S/m

Show Material materials with Electrical conductivity of 35800000.0 - 36800000.0 S/m

H111

EN 573-3

Flat

Electrical resistivity

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m

H111

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Tube, Bar

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.7 %

Show Material materials with Aluminium of 99.7 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

Copper

0.03 %

Show Material materials with Copper of 0.03 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.03 %

Show Material materials with Copper of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Iron

0.25 %

Show Material materials with Iron of 0.25 %

H111

EN 573-3

Flat

0.25 %

Show Material materials with Iron of 0.25 %

H111

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Wire, Tube, Bar, Coil, Sheet, Strip

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.03 %

Show Material materials with Magnesium of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.03 %

Show Material materials with Manganese of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Other

0.03 %

Show Material materials with Other of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Min.

Silicon

0.2 %

Show Material materials with Silicon of 0.2 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.2 %

Show Material materials with Silicon of 0.2 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.03 %

Show Material materials with Titanium of 0.03 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Zinc

0.07 %

Show Material materials with Zinc of 0.07 %

H111

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire, Tube, Bar

0.07 %

Show Material materials with Zinc of 0.07 %

H111

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetic pieces; Automotive trim: Interior trim, Windows frame, Marque badges

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent