General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H111 | EN 573-3 | Sheet, Flat, Strip, Tube |
Dimension
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Thickness | 0.2 mm Show Material materials with Thickness of 0.2 mm | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | 0.2 mm | Plate, Sheet, Strip |
6.0 mm Show Material materials with Thickness of 6.0 mm | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | 6.0 mm | Plate, Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 180° | 0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |||
1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
Bending angle 90° | 0 °/t Show Material materials with Bending angle 90° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | ||
0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
Elastic modulus | -270 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip, Flat | ||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H111 | EN 573-3 | Sheet, Flat, Strip, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Elastic modulus of 68.0 GPa | H111 | EN 573-3 | Sheet, Flat, Strip, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Elastic modulus of 66.0 GPa | H111 | EN 573-3 | Sheet, Flat, Strip, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Elastic modulus of 63.0 GPa | H111 | EN 573-3 | Sheet, Flat, Strip, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Elastic modulus of 57.0 GPa | H111 | EN 573-3 | Sheet, Flat, Strip, Tube | ||
300 °C | 50.0 GPa Show Material materials with Elastic modulus of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Elastic modulus of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Flat | ||
Elongation | 12.0 % Show Material materials with Elongation of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | |
12.0 - 18.0 % Show Material materials with Elongation of 12.0 - 18.0 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | A50 | ||
14.0 % Show Material materials with Elongation of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
15.0 % Show Material materials with Elongation of 15.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
16.0 % Show Material materials with Elongation of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
17.0 % Show Material materials with Elongation of 17.0 % | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | H111 | EN 573-3 | Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | H111 | EN 573-3 | Tube, Flat | ||
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Flat | A50 | |
Hardness, Brinell | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
52.0 [-] Show Material materials with Hardness, Brinell of 52.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | H111 | EN 573-3 | Tube | ||
20.0 °C | 52.0 [-] Show Material materials with Hardness, Brinell of 52.0 [-] | H111 | EN 573-3 | Flat | ||
Hardness, HBW | 52 [-] Show Material materials with Hardness, HBW of 52 [-] | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | ||
Impact strength, Charpy notched | 30.0 kJ/m² Show Material materials with Impact strength, Charpy notched of 30.0 kJ/m² | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | H111 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Flat, Strip, Tube, Plate, Sheet, Strip | |
Tensile strength | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | H111 | EN 573-3 | Tube | ||
20.0 °C | 180.0 - 250.0 MPa Show Material materials with Tensile strength of 180.0 - 250.0 MPa | H111 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Tensile strength of 190.0 - 240.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | H111 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Tensile strength of 190.0 - 240.0 MPa | H111 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Flat, Sheet, Strip | ||
Yield strength | -270 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Sheet, Strip, Tube, Plate, Rod, Welded Tube, Flat | RP02 |
-270.0 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Sheet, Strip, Tube, Plate, Rod, Welded Tube, Flat | RP02 | |
80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | RP02 | ||
80 MPa Show Material materials with Yield strength of 80 MPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |||
20.0 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Sheet, Strip, Tube, Plate, Rod, Welded Tube, Flat | RP02 | |
20 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Sheet, Strip, Tube, Plate, Rod, Welded Tube, Flat | RP02 | |
50.0 °C | 80.0 MPa Show Material materials with Yield strength of 80.0 MPa | H111 | EN 573-3 | Sheet, Strip, Tube, Plate, Rod, Welded Tube, Flat | RP02 | |
100 °C | 70.0 MPa Show Material materials with Yield strength of 70.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | RP02 | |
100.0 °C | 70.0 MPa Show Material materials with Yield strength of 70.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Coefficient of thermal expansion of 0.000024 1/K | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | 20-100°C | |
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | H111 | EN 573-3 | Flat, Tube | Long | |
150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Melting point | 620.0 - 650.0 °C Show Material materials with Melting point of 620.0 - 650.0 °C | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Specific heat capacity | 879.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Thermal conductivity | 147 W/(m·K) Show Material materials with Thermal conductivity of 147 W/(m·K) | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | ||
20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K) | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
Electrical resistivity | 4e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
4.4e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 4.4e-08 - 5e-08 Ω·m | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
0.3 % Show Material materials with Chromium of 0.3 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
0.1 % Show Material materials with Copper of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
0.3 % Show Material materials with Copper of 0.3 % | H111 | EN 573-3 | Flat | |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | H111 | EN 573-3 | Sheet, Flat, Strip, Tube |
0.50 % Show Material materials with Iron of 0.50 % | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
0.5 % Show Material materials with Iron of 0.5 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
0.7 % Show Material materials with Iron of 0.7 % | H111 | EN 573-3 | Flat | |
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H111 | EN 573-3, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube, Sheet, Strip |
1.6 - 2.6 % Show Material materials with Magnesium of 1.6 - 2.6 % | H111 | EN 573-3 | Flat | |
Manganese | 0.5 - 1.1 % Show Material materials with Manganese of 0.5 - 1.1 % | H111 | EN 573-3, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube, Sheet, Strip |
0.6 - 1.1 % Show Material materials with Manganese of 0.6 - 1.1 % | H111 | EN 573-3 | Flat | |
Other | 0.05 - 0.15 % Show Material materials with Other of 0.05 - 0.15 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
0.4 % Show Material materials with Silicon of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
0.1 % Show Material materials with Titanium of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H111 | EN 573-3, EN 485, EN 754 | Sheet, Flat, Strip, Tube, Plate, Rod, Welded Tube |
0.2 % Show Material materials with Zinc of 0.2 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Plate, Sheet, Strip | |
0.3 % Show Material materials with Zinc of 0.3 % | H111 | EN 573-3 | Flat |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Application areas | Components: General trasportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |