General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Sheet | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Density of 2.68 - 2.69 g/cm³ | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 2.69 g/cm³ Show Material materials with Density of 2.69 g/cm³ | O | EN 573-3 | Rod, Flat, Tube, Wire |
Dimension
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Bending angle 180° | 0 °/t Show Material materials with Bending angle 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Bending angle 90° | 0 °/t Show Material materials with Bending angle 90° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Sheet | ||
Elongation | -196.0 °C | 46.0 % Show Material materials with Elongation of 46.0 % | O | EN 573-3 | ||
-80.0 °C | 35.0 % Show Material materials with Elongation of 35.0 % | O | EN 573-3 | |||
-28.0 °C | 32.0 % Show Material materials with Elongation of 32.0 % | O | EN 573-3 | |||
12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
12 % Show Material materials with Elongation of 12 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | A50 | ||
14.0 % Show Material materials with Elongation of 14.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongation of 15.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
15.0 % Show Material materials with Elongation of 15.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongation of 17.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongation of 17.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
19.0 % Show Material materials with Elongation of 19.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongation of 20.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 19.0 % Show Material materials with Elongation of 19.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongation of 19.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 30.0 % Show Material materials with Elongation of 30.0 % | O | EN 573-3 | |||
100.0 °C | 35.0 % Show Material materials with Elongation of 35.0 % | O | EN 573-3 | |||
150.0 °C | 50.0 % Show Material materials with Elongation of 50.0 % | O | EN 573-3 | |||
200.0 °C | 60.0 % Show Material materials with Elongation of 60.0 % | O | EN 573-3 | |||
260.0 °C | 80.0 % Show Material materials with Elongation of 80.0 % | O | EN 573-3 | |||
315.0 °C | 110.0 % Show Material materials with Elongation of 110.0 % | O | EN 573-3 | |||
370.0 °C | 130.0 % Show Material materials with Elongation of 130.0 % | O | EN 573-3 | |||
Hardness, Brinell | 46.0 [-] Show Material materials with Hardness, Brinell of 46.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
47.0 [-] Show Material materials with Hardness, Brinell of 47.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 46.0 - 47.0 [-] Show Material materials with Hardness, Brinell of 46.0 - 47.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 46.0 [-] Show Material materials with Hardness, Brinell of 46.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 47.0 [-] Show Material materials with Hardness, Brinell of 47.0 [-] | O | EN 573-3 | Rod, Tube, Flat | ||
Hardness, HBW | 47 [-] Show Material materials with Hardness, HBW of 47 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 20.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | O | EN 573-3 | Rod, Flat, Tube, Wire | |
Shear modulus | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Shear modulus of 26.3 - 27.0 GPa | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Tensile strength | -196.0 °C | 300.0 MPa Show Material materials with Tensile strength of 300.0 MPa | O | EN 573-3 | ||
-80.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | O | EN 573-3 | |||
-28.0 °C | 195.0 MPa Show Material materials with Tensile strength of 195.0 MPa | O | EN 573-3 | |||
225.0 MPa Show Material materials with Tensile strength of 225.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Tensile strength of 165.0 - 215.0 MPa | O | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Tensile strength of 165.0 - 215.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Tensile strength of 170.0 MPa | O | EN 573-3 | Rod | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Tensile strength of 170.0 - 230.0 MPa | O | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Tensile strength of 170.0 - 215.0 MPa | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Tensile strength of 170.0 - 215.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 195.0 MPa Show Material materials with Tensile strength of 195.0 MPa | O | EN 573-3 | |||
20.0 °C | 225.0 MPa Show Material materials with Tensile strength of 225.0 MPa | O | EN 573-3 | Wire | ||
100.0 °C | 195.0 MPa Show Material materials with Tensile strength of 195.0 MPa | O | EN 573-3 | |||
150.0 °C | 160.0 MPa Show Material materials with Tensile strength of 160.0 MPa | O | EN 573-3 | |||
200.0 °C | 115.0 MPa Show Material materials with Tensile strength of 115.0 MPa | O | EN 573-3 | |||
260.0 °C | 85.0 MPa Show Material materials with Tensile strength of 85.0 MPa | O | EN 573-3 | |||
315.0 °C | 50.0 MPa Show Material materials with Tensile strength of 50.0 MPa | O | EN 573-3 | |||
370.0 °C | 35.0 MPa Show Material materials with Tensile strength of 35.0 MPa | O | EN 573-3 | |||
Yield strength | -196.0 °C | 110.0 MPa Show Material materials with Yield strength of 110.0 MPa | O | EN 573-3 | RP02 | |
-80.0 °C | 90.0 MPa Show Material materials with Yield strength of 90.0 MPa | O | EN 573-3 | RP02 | ||
-28.0 °C | 90.0 MPa Show Material materials with Yield strength of 90.0 MPa | O | EN 573-3 | RP02 | ||
65.0 MPa Show Material materials with Yield strength of 65.0 MPa | O | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
65 MPa Show Material materials with Yield strength of 65 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
70.0 MPa Show Material materials with Yield strength of 70.0 MPa | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
100.0 MPa Show Material materials with Yield strength of 100.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
20.0 °C | 65.0 MPa Show Material materials with Yield strength of 65.0 MPa | O | EN 573-3 | Rod, Tube, Flat | RP02 | |
20.0 °C | 65.0 MPa Show Material materials with Yield strength of 65.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Yield strength of 70.0 MPa | O | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Yield strength of 90.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 100.0 MPa Show Material materials with Yield strength of 100.0 MPa | O | EN 573-3 | Wire | RP02 | |
100.0 °C | 90.0 MPa Show Material materials with Yield strength of 90.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 90.0 MPa Show Material materials with Yield strength of 90.0 MPa | O | EN 573-3 | RP02 | ||
200.0 °C | 75.0 MPa Show Material materials with Yield strength of 75.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 50.0 MPa Show Material materials with Yield strength of 50.0 MPa | O | EN 573-3 | RP02 | ||
315.0 °C | 40.0 MPa Show Material materials with Yield strength of 40.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 20.0 MPa Show Material materials with Yield strength of 20.0 MPa | O | EN 573-3 | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50.0 °C | 2.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.21e-05 1/K | O | EN 573-3 | Rod, Flat, Tube, Wire | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Coefficient of thermal expansion of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | 20-100°C | |
200 °C | 2.48e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.57e-05 1/K | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 605.0 - 650.0 °C Show Material materials with Melting point of 605.0 - 650.0 °C | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Melting point of 607.0 - 649.0 °C | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 - 901.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Specific heat capacity of 901.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Thermal conductivity | 138 W/(m·K) Show Material materials with Thermal conductivity of 138 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 138.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 138.0 - 150.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Thermal conductivity of 138.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
Electrical resistivity | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
4.9e-08 Ω·m Show Material materials with Electrical resistivity of 4.9e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
5e-08 Ω·m Show Material materials with Electrical resistivity of 5e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with Electrical resistivity of 4.7e-08 - 4.95e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with Electrical resistivity of 4.7e-08 - 5.2e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with Electrical resistivity of 4.95e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with Electrical resistivity of 4.95e-08 - 5.2e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.15 - 0.35 % Show Material materials with Chromium of 0.15 - 0.35 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Copper of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Iron | 0.4 % Show Material materials with Iron of 0.4 % | O | EN 573-3 | Rod, Flat, Tube, Wire |
0.40 % Show Material materials with Iron of 0.40 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.4 % Show Material materials with Iron of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Manganese of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Other | 0.15 % Show Material materials with Other of 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.25 % Show Material materials with Silicon of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |