EN 573-3 Grade AW-5086 O

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5086 is structural alloy, which offers users strong corrosion resistance and high electrical conductivity. Offering higher strength levels than 5052 or 5083, EN AW-5086 becomes stronger with stain hardening and cold working, all while remaining a cost-effective choice. It can be welded with conventional methods, though electric arc welding is preferred.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate

20.0 °C

2.66 - 2.67 g/cm³

Show Material materials with Density of 2.66 - 2.67 g/cm³

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

2.67 g/cm³

Show Material materials with Density of 2.67 g/cm³

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Plate

6.0 mm

Show Material materials with Thickness of 6.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

6.0 mm

Coil, Sheet, Plate

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

120.0 MPa

Show Material materials with Bending Fatigue Strength of 120.0 MPa

O

EN 573-3, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

1 °/t

Show Material materials with Bending angle 180° of 1 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

O

EN 573-3, EN 14286, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

3.0 °/t

Show Material materials with Bending angle 180° of 3.0 °/t

O

EN 573-3, EN 14286

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate

Elongation

-196.0 °C

46.0 %

Show Material materials with Elongation of 46.0 %

O

EN 573-3

-80.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

O

EN 573-3

-28.0 °C

32.0 %

Show Material materials with Elongation of 32.0 %

O

EN 573-3

11.0 %

Show Material materials with Elongation of 11.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

11.0 - 15.0 %

Show Material materials with Elongation of 11.0 - 15.0 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

A50

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 1592

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A50

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3, EN 14286

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 14286, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

A100

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

O

EN 573-3

Flat

A50

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Flat

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Seamless Tube

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Rod, Tube, Flat

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3

Flat

A50

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Rod, Tube

20.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

100.0 °C

36.0 %

Show Material materials with Elongation of 36.0 %

O

EN 573-3

150.0 °C

50.0 %

Show Material materials with Elongation of 50.0 %

O

EN 573-3

200.0 °C

60.0 %

Show Material materials with Elongation of 60.0 %

O

EN 573-3

260.0 °C

80.0 %

Show Material materials with Elongation of 80.0 %

O

EN 573-3

315.0 °C

110.0 %

Show Material materials with Elongation of 110.0 %

O

EN 573-3

370.0 °C

130.0 %

Show Material materials with Elongation of 130.0 %

O

EN 573-3

Unlock all property charts

Hardness, Brinell

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

O

EN 573-3

Rod, Flat, Tube

Hardness, HBW

65 [-]

Show Material materials with Hardness, HBW of 65 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Shear modulus

26.7 GPa

Show Material materials with Shear modulus of 26.7 GPa

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

27.0 GPa

Show Material materials with Shear modulus of 27.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

20.0 °C

26.7 - 27.0 GPa

Show Material materials with Shear modulus of 26.7 - 27.0 GPa

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

26.7 GPa

Show Material materials with Shear modulus of 26.7 GPa

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Unlock all property charts

Tensile strength

-196.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

O

EN 573-3

-80.0 °C

270.0 MPa

Show Material materials with Tensile strength of 270.0 MPa

O

EN 573-3

-28.0 °C

260.0 MPa

Show Material materials with Tensile strength of 260.0 MPa

O

EN 573-3

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

O

EN 573-3, EN 1592

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

240.0 - 320.0 MPa

Show Material materials with Tensile strength of 240.0 - 320.0 MPa

O

EN 573-3, EN 754, EN 755

Rod, Tube, Strip, Sheet, Plate, Welded Tube, Wire

20.0 °C

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

O

EN 573-3

Seamless Tube

20.0 °C

240.0 - 310.0 MPa

Show Material materials with Tensile strength of 240.0 - 310.0 MPa

O

EN 573-3, EN 14286, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate

20.0 °C

240.0 - 310.0 MPa

Show Material materials with Tensile strength of 240.0 - 310.0 MPa

O

EN 573-3

Flat

Transverse

20.0 °C

260.0 MPa

Show Material materials with Tensile strength of 260.0 MPa

O

EN 573-3

100.0 °C

260.0 MPa

Show Material materials with Tensile strength of 260.0 MPa

O

EN 573-3

150.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

O

EN 573-3

200.0 °C

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

O

EN 573-3

260.0 °C

115.0 MPa

Show Material materials with Tensile strength of 115.0 MPa

O

EN 573-3

315.0 °C

75.0 MPa

Show Material materials with Tensile strength of 75.0 MPa

O

EN 573-3

370.0 °C

40.0 MPa

Show Material materials with Tensile strength of 40.0 MPa

O

EN 573-3

Unlock all property charts

Yield strength

-196.0 °C

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

O

EN 573-3

RP02

-80.0 °C

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

O

EN 573-3

RP02

-28.0 °C

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

O

EN 573-3

RP02

95.0 MPa

Show Material materials with Yield strength of 95.0 MPa

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

RP02

100.0 MPa

Show Material materials with Yield strength of 100.0 MPa

O

EN 573-3, EN 14286, EN 1592, EN 485

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

RP02

100 MPa

Show Material materials with Yield strength of 100 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

20.0 °C

95.0 MPa

Show Material materials with Yield strength of 95.0 MPa

O

EN 573-3

Rod, Tube

RP02

20.0 °C

100.0 MPa

Show Material materials with Yield strength of 100.0 MPa

O

EN 573-3

Seamless Tube, Flat

RP02

20.0 °C

100.0 MPa

Show Material materials with Yield strength of 100.0 MPa

O

EN 573-3

Flat

RP02 Transverse

20.0 °C

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

O

EN 573-3

RP02

100.0 °C

115.0 MPa

Show Material materials with Yield strength of 115.0 MPa

O

EN 573-3

RP02

150.0 °C

110.0 MPa

Show Material materials with Yield strength of 110.0 MPa

O

EN 573-3

RP02

200.0 °C

105.0 MPa

Show Material materials with Yield strength of 105.0 MPa

O

EN 573-3

RP02

260.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

O

EN 573-3

RP02

315.0 °C

50.0 MPa

Show Material materials with Yield strength of 50.0 MPa

O

EN 573-3

RP02

370.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

RP02

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

-50.0 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

20 °C

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

100.0 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

20-100°C

200 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

200.0 °C

2.47e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.47e-05 1/K

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

300 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

300.0 °C

2.58e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

Unlock all property charts

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

585.0 - 641.0 °C

Show Material materials with Melting point of 585.0 - 641.0 °C

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

585.0 - 640.0 °C

Show Material materials with Melting point of 585.0 - 640.0 °C

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Thermal conductivity

126 W/(m·K)

Show Material materials with Thermal conductivity of 126 W/(m·K)

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate

20.0 °C

120.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 140.0 W/(m·K)

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

20.0 °C

120.0 - 126.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 - 126.0 W/(m·K)

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

126.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 126.0 - 140.0 W/(m·K)

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

126.0 W/(m·K)

Show Material materials with Thermal conductivity of 126.0 W/(m·K)

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

18000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 S/m

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

17000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 19000000.0 S/m

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube

Electrical resistivity

5.26e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 5.88e-08 Ω·m

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 5.56e-08 Ω·m

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

20.0 °C

5.2e-08 - 5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 5.6e-08 Ω·m

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

5.2e-08 - 5.8e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 5.8e-08 Ω·m

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

20.0 °C

5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.6e-08 Ω·m

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate

20.0 °C

5.6e-08 - 5.8e-08 Ω·m

Show Material materials with Electrical resistivity of 5.6e-08 - 5.8e-08 Ω·m

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate

Copper

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Iron

0.5 %

Show Material materials with Iron of 0.5 %

O

EN 573-3

Rod, Flat, Seamless Tube, Tube

0.50 %

Show Material materials with Iron of 0.50 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire

0.5 %

Show Material materials with Iron of 0.5 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Magnesium

3.5 - 4.5 %

Show Material materials with Magnesium of 3.5 - 4.5 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate

Manganese

0.2 - 0.7 %

Show Material materials with Manganese of 0.2 - 0.7 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate

Other

0.05 - 0.15 %

Show Material materials with Other of 0.05 - 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire

0.4 %

Show Material materials with Silicon of 0.4 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire

0.15 %

Show Material materials with Titanium of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Plate

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Vessels: Pressure, Cryogenics; Components: Access hatches, Spoilers, General tranportation

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Excellent

Welding

Good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)