EN 573-3 Grade AW-5454 H112

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

2.68 - 2.69 g/cm³

Show Material materials with Density of 2.68 - 2.69 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

70.5 GPa

Show Material materials with Elastic modulus of 70.5 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Elongation

8.0 %

Show Material materials with Elongation of 8.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

13.0 %

Show Material materials with Elongation of 13.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

A50

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H112

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H112

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H112

EN 573-3

Flat

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H112

EN 573-3

Flat

Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

H112

EN 573-3

Sheet

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

H112

EN 573-3

Flat

Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Profile, Rod, Tube

Hardness, Brinell

59.0 [-]

Show Material materials with Hardness, Brinell of 59.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

20.0 °C

59.0 [-]

Show Material materials with Hardness, Brinell of 59.0 [-]

H112

EN 573-3

Sheet, Flat

20.0 °C

59.0 - 63.0 [-]

Show Material materials with Hardness, Brinell of 59.0 - 63.0 [-]

H112

EN 573-3

Flat

20.0 °C

60.0 [-]

Show Material materials with Hardness, Brinell of 60.0 [-]

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

63.0 [-]

Show Material materials with Hardness, Brinell of 63.0 [-]

H112

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

26.5 - 27.0 GPa

Show Material materials with Shear modulus of 26.5 - 27.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Tensile strength

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

215.0 MPa

Show Material materials with Tensile strength of 215.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

215.0 MPa

Show Material materials with Tensile strength of 215.0 MPa

H112

EN 573-3

Sheet, Flat

20.0 °C

215.0 MPa

Show Material materials with Tensile strength of 215.0 MPa

H112

EN 573-3

Flat

Transverse

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H112

EN 573-3

Flat

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H112

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.1899999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1899999999999997e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

-50.0 °C

2.19e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.19e-05 1/K

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20 °C

2.1899999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1899999999999997e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

20 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

100.0 °C

2.37e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.37e-05 1/K

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

200 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

200.0 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

300 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

300.0 °C

2.56e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

602.0 - 646.0 °C

Show Material materials with Melting point of 602.0 - 646.0 °C

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

897.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 - 900.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Thermal conductivity

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

135.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 135.0 - 150.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

20.0 °C

135.0 W/(m·K)

Show Material materials with Thermal conductivity of 135.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

19000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

21000000.0 S/m

Show Material materials with Electrical conductivity of 21000000.0 S/m

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Electrical resistivity

4.76e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

5.1e-08 Ω·m

Show Material materials with Electrical resistivity of 5.1e-08 Ω·m

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.2 %

Show Material materials with Chromium of 0.05 - 0.2 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H112

EN 573-3

Profile, Rod, Flat, Tube, Sheet

0.40 %

Show Material materials with Iron of 0.40 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

Magnesium

2.4 - 3.0 %

Show Material materials with Magnesium of 2.4 - 3.0 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Manganese

0.5 - 1.0 %

Show Material materials with Manganese of 0.5 - 1.0 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H112

EN 573-3, EN 13195, EN 485, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability