General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Bending angle 180° | 1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
2.0 °/t Show Material materials with Bending angle 180° of 2.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Bending angle 90° | 1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
3.0 °/t Show Material materials with Bending angle 90° of 3.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | T4 | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 68.3 - 69.6 GPa Show Material materials with Elastic modulus of 68.3 - 69.6 GPa | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | ||
Elongation | 6.0 % Show Material materials with Elongation of 6.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | |
8.0 % Show Material materials with Elongation of 8.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
10.0 % Show Material materials with Elongation of 10.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongation of 15.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Elongation of 18.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3 | Plate, Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3 | Plate | ||
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3 | Wire | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3 | Sheet | ||
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | T4 | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
Hardness, Brinell | 58.0 [-] Show Material materials with Hardness, Brinell of 58.0 [-] | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 58.0 [-] Show Material materials with Hardness, Brinell of 58.0 [-] | T4 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | T4 | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 26.2 GPa Show Material materials with Shear modulus of 26.2 GPa | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | ||
Tensile strength | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
205.0 MPa Show Material materials with Tensile strength of 205.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
250.0 - 280.0 MPa Show Material materials with Tensile strength of 250.0 - 280.0 MPa | T4 | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | T4 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 205.0 MPa Show Material materials with Tensile strength of 205.0 MPa | T4 | EN 573-3 | Rod, Tube, Wire, Sheet, Plate, Flat | ||
20.0 °C | 205.0 MPa Show Material materials with Tensile strength of 205.0 MPa | T4 | EN 573-3 | Flat | Transverse |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar |
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Melting point | 580.0 - 640.0 °C Show Material materials with Melting point of 580.0 - 640.0 °C | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
580.0 - 650.0 °C Show Material materials with Melting point of 580.0 - 650.0 °C | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Specific heat capacity | 20.0 °C | 870.0 J/(kg·K) Show Material materials with Specific heat capacity of 870.0 J/(kg·K) | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
Thermal conductivity | 155.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 155.0 - 180.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
170.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 200.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 150.0 - 165.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 - 165.0 W/(m·K) | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 22000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 22000000.0 - 30000000.0 S/m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
23000000.0 - 27000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 27000000.0 S/m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 20000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 30000000.0 S/m | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | |
Electrical resistivity | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with Electrical resistivity of 3.33e-08 - 4.55e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
3.7e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.7e-08 - 4.35e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.04 - 0.35 % Show Material materials with Chromium of 0.04 - 0.35 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
0.70 % Show Material materials with Iron of 0.70 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |