General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Density | 20.0 °C | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ | F53 | EN 573-3 |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 70.0 - 73.0 GPa Show Material materials with Elastic modulus of 70.0 - 73.0 GPa | F53 | EN 573-3 | |
Elongation | -196.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | F53 | EN 573-3 | |
-80.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | F53 | EN 573-3 | ||
-28.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | F53 | EN 573-3 | ||
20.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | F53 | EN 573-3 | ||
100.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | F53 | EN 573-3 | ||
150.0 °C | 30.0 % Show Material materials with Elongation of 30.0 % | F53 | EN 573-3 | ||
200.0 °C | 55.0 % Show Material materials with Elongation of 55.0 % | F53 | EN 573-3 | ||
260.0 °C | 65.0 % Show Material materials with Elongation of 65.0 % | F53 | EN 573-3 | ||
315.0 °C | 70.0 % Show Material materials with Elongation of 70.0 % | F53 | EN 573-3 | ||
370.0 °C | 70.0 % Show Material materials with Elongation of 70.0 % | F53 | EN 573-3 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | |||
Shear modulus | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Shear modulus of 25.0 - 27.0 GPa | F53 | EN 573-3 | |
Tensile strength | -196.0 °C | 700.0 MPa Show Material materials with Tensile strength of 700.0 MPa | F53 | EN 573-3 | |
-80.0 °C | 620.0 MPa Show Material materials with Tensile strength of 620.0 MPa | F53 | EN 573-3 | ||
-28.0 °C | 590.0 MPa Show Material materials with Tensile strength of 590.0 MPa | F53 | EN 573-3 | ||
20.0 °C | 570.0 MPa Show Material materials with Tensile strength of 570.0 MPa | F53 | EN 573-3 | ||
100.0 °C | 485.0 MPa Show Material materials with Tensile strength of 485.0 MPa | F53 | EN 573-3 | ||
150.0 °C | 215.0 MPa Show Material materials with Tensile strength of 215.0 MPa | F53 | EN 573-3 | ||
200.0 °C | 110.0 MPa Show Material materials with Tensile strength of 110.0 MPa | F53 | EN 573-3 | ||
260.0 °C | 75.0 MPa Show Material materials with Tensile strength of 75.0 MPa | F53 | EN 573-3 | ||
315.0 °C | 55.0 MPa Show Material materials with Tensile strength of 55.0 MPa | F53 | EN 573-3 | ||
370.0 °C | 40.0 MPa Show Material materials with Tensile strength of 40.0 MPa | F53 | EN 573-3 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50.0 °C | 2.16e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K | F53 | EN 573-3 | |
100.0 °C | 2.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.34e-05 1/K | F53 | EN 573-3 | ||
200.0 °C | 2.43e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K | F53 | EN 573-3 | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K | F53 | EN 573-3 | ||
Melting point | 465.0 - 655.0 °C Show Material materials with Melting point of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium | |||
Specific heat capacity | 20.0 °C | 862.0 J/(kg·K) Show Material materials with Specific heat capacity of 862.0 J/(kg·K) | F53 | EN 573-3 | |
Thermal conductivity | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K) | F53 | EN 573-3 |
Electrical
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m | F53 | EN 573-3 | |
Electrical resistivity | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.18 - 0.28 % Show Material materials with Chromium of 0.18 - 0.28 % | F53 | EN 573-3 |
Copper | 1.2 - 2.0 % Show Material materials with Copper of 1.2 - 2.0 % | F53 | EN 573-3 |
Iron | 0.5 Show Material materials with Iron of 0.5 | F53 | EN 573-3 |
Magnesium | 2.1 - 2.9 % Show Material materials with Magnesium of 2.1 - 2.9 % | F53 | EN 573-3 |
Manganese | 0.3 Show Material materials with Manganese of 0.3 | F53 | EN 573-3 |
Silicon | 0.4 Show Material materials with Silicon of 0.4 | F53 | EN 573-3 |
Titanium | 0.2 Show Material materials with Titanium of 0.2 | F53 | EN 573-3 |
Zinc | 5.1 - 6.1 % Show Material materials with Zinc of 5.1 - 6.1 % | F53 | EN 573-3 |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |