General
Property | Value | Comment |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | Typical for Wrought 4000 Series Aluminium |
Mechanical
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastic modulus | 69.0 - 71.0 GPa Show Material materials with Elastic modulus of 69.0 - 71.0 GPa | Typical for Wrought 4000 Series Aluminium | |||
Elongation | 3.0 % Show Material materials with Elongation of 3.0 % | T86 | ASTM B211 | Bar, Rod, Wire | |
4.0 % Show Material materials with Elongation of 4.0 % | T86 | ASTM B211 | Bar, Rod, Wire | A50 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 4000 Series Aluminium | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 4000 Series Aluminium | |||
Shear modulus | 26.0 GPa Show Material materials with Shear modulus of 26.0 GPa | Typical for Wrought 4000 Series Aluminium | |||
Tensile strength | 350.0 MPa Show Material materials with Tensile strength of 350.0 MPa | T86 | ASTM B211 | Bar, Rod, Wire |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.2e-05 - 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.2e-05 - 2.2e-05 1/K | Typical for Wrought 4000 Series Aluminium |
Melting point | 520.0 - 630.0 °C Show Material materials with Melting point of 520.0 - 630.0 °C | Typical for Wrought 4000 Series Aluminium |
Specific heat capacity | 864.0 J/(kg·K) Show Material materials with Specific heat capacity of 864.0 J/(kg·K) | Typical for Wrought 4000 Series Aluminium |
Thermal conductivity | 138.0 - 155.0 W/(m·K) Show Material materials with Thermal conductivity of 138.0 - 155.0 W/(m·K) | Typical for Wrought 4000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 23000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 30000000.0 S/m | Typical for Wrought 4000 Series Aluminium |
Electrical resistivity | 3.8e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 3.8e-08 - 5e-08 Ω·m | Typical for Wrought 4000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 Show Material materials with Chromium of 0.1 | T86 | ASTM B211 | Bar, Rod, Wire |
Copper | 0.5 - 1.3 % Show Material materials with Copper of 0.5 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Iron | 1.0 Show Material materials with Iron of 1.0 | T86 | ASTM B211 | Bar, Rod, Wire |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Nickel | 0.5 - 1.3 % Show Material materials with Nickel of 0.5 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Silicon | 11.0 - 13.5 % Show Material materials with Silicon of 11.0 - 13.5 % | T86 | ASTM B211 | Bar, Rod, Wire |
Zinc | 0.25 Show Material materials with Zinc of 0.25 | T86 | ASTM B211 | Bar, Rod, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |