Aluminum EN AW-2024, known for its use in aircraft industry, is an alloy that offers excellent strength. When in the annealed condition it is readily formed and has good machinability. Though it has a relatively low level of corrosion resistance, it can be machined to a high finish.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T351

EN 573-3

Rod, Sheet, Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

4.0 °/t

Show Material materials with Bending angle 180° of 4.0 °/t

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

5.0 °/t

Show Material materials with Bending angle 180° of 5.0 °/t

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Bending angle 90°

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

8.0 °/t

Show Material materials with Bending angle 90° of 8.0 °/t

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

70.0 - 74.5 GPa

Show Material materials with Elastic modulus of 70.0 - 74.5 GPa

T351

EN 573-3

Rod, Sheet, Flat

Elongation

5.0 %

Show Material materials with Elongation of 5.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T351

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T351

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

11.0 %

Show Material materials with Elongation of 11.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

12.0 %

Show Material materials with Elongation of 12.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

13.0 %

Show Material materials with Elongation of 13.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

14.0 %

Show Material materials with Elongation of 14.0 %

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T351

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T351

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T351

EN 573-3

Rod

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T351

EN 573-3

Sheet

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T351

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T351

EN 573-3

Rod, Sheet

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T351

EN 573-3

Flat

Transverse

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T351

EN 573-3

Flat

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T351

EN 573-3

Sheet, Flat

Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T351

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T351

EN 573-3

Flat

A50 Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T351

EN 573-3

Flat

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T351

EN 573-3

Sheet, Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T351

EN 573-3

Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T351

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

115.0 [-]

Show Material materials with Hardness, Brinell of 115.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

120.0 [-]

Show Material materials with Hardness, Brinell of 120.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

122.0 [-]

Show Material materials with Hardness, Brinell of 122.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

124.0 [-]

Show Material materials with Hardness, Brinell of 124.0 [-]

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

104.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 120.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 115.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 115.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 110.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 110.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

104.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

104.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 122.0 [-]

T351

EN 573-3

Flat

20.0 °C

110.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 120.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

110.0 - 115.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 115.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

110.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

110.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

110.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 122.0 [-]

T351

EN 573-3

Flat

20.0 °C

115.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 120.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

115.0 [-]

Show Material materials with Hardness, Brinell of 115.0 [-]

T351

EN 573-3

Sheet, Flat

20.0 °C

115.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

115.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

115.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 122.0 [-]

T351

EN 573-3

Flat

20.0 °C

120.0 [-]

Show Material materials with Hardness, Brinell of 120.0 [-]

T351

EN 573-3

Rod, Sheet, Flat

20.0 °C

120.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

120.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

120.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 122.0 [-]

T351

EN 573-3

Flat

20.0 °C

122.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 122.0 - 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

122.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 122.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

122.0 [-]

Show Material materials with Hardness, Brinell of 122.0 [-]

T351

EN 573-3

Flat

20.0 °C

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T351

EN 573-3

Flat

20.0 °C

123.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 124.0 [-]

T351

EN 573-3

Flat

20.0 °C

124.0 [-]

Show Material materials with Hardness, Brinell of 124.0 [-]

T351

EN 573-3

Flat

Plane-Strain Fracture Toughnes

20.0 °C

26.0 - 36.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 36.0 MPa·√m

T351

EN 573-3

Sheet

20.0 °C

26.0 - 33.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 33.0 MPa·√m

T351

EN 573-3

Sheet

20.0 °C

26.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 26.0 MPa·√m

T351

EN 573-3

Sheet

20.0 °C

33.0 - 36.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 36.0 MPa·√m

T351

EN 573-3

Sheet

20.0 °C

33.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 33.0 MPa·√m

T351

EN 573-3

Sheet

20.0 °C

36.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 36.0 MPa·√m

T351

EN 573-3

Sheet

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

27.0 - 28.0 GPa

Show Material materials with Shear modulus of 27.0 - 28.0 GPa

T351

EN 573-3

Rod, Sheet, Flat

Tensile strength

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T351

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

T351

EN 573-3

Sheet

Transverse

20.0 °C

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T351

EN 573-3

Sheet

20.0 °C

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T351

EN 573-3

Sheet

20.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T351

EN 573-3

Sheet

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T351

EN 573-3

Sheet

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T351

EN 573-3

Rod

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T351

EN 573-3

Flat

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T351

EN 573-3

Flat

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T351

EN 573-3

Flat

Transverse

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T351

EN 573-3

Flat

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T351

EN 573-3

Flat

Transverse

Yield strength

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T351

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

310.0 MPa

Show Material materials with Yield strength of 310.0 MPa

T351

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

20.0 °C

140.0 MPa

Show Material materials with Yield strength of 140.0 MPa

T351

EN 573-3

Sheet

RP02 Transverse

20.0 °C

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T351

EN 573-3

Sheet

RP02

20.0 °C

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T351

EN 573-3

Flat

RP02 Transverse

20.0 °C

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T351

EN 573-3

Sheet

RP02

20.0 °C

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T351

EN 573-3

Flat

RP02 Transverse

20.0 °C

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T351

EN 573-3

Sheet

RP02

20.0 °C

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T351

EN 573-3

Flat

RP02 Transverse

20.0 °C

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T351

EN 573-3

Sheet, Flat

RP02

20.0 °C

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T351

EN 573-3

Flat

RP02 Transverse

20.0 °C

310.0 MPa

Show Material materials with Yield strength of 310.0 MPa

T351

EN 573-3

Rod

RP02

20.0 °C

325.0 MPa

Show Material materials with Yield strength of 325.0 MPa

T351

EN 573-3

Sheet

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

200 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

300 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Melting point

505.0 - 640.0 °C

Show Material materials with Melting point of 505.0 - 640.0 °C

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T351

EN 573-3

Rod, Sheet, Flat

Thermal conductivity

121.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K)

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

T351

EN 573-3, EN 485, EN 754

Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Welded Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

17000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

18000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m

T351

EN 573-3, EN 485, EN 754

Rod, Sheet, Flat, Strip, Plate, Forging, Tube, Welded Tube, Bar

Electrical resistivity

3.45e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

4.76e-08 - 5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Copper

3.8 - 4.9 %

Show Material materials with Copper of 3.8 - 4.9 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T351

EN 573-3

Sheet, Flat, Rod

0.50 %

Show Material materials with Iron of 0.50 %

T351

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

1.2 - 1.8 %

Show Material materials with Magnesium of 1.2 - 1.8 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Manganese

0.3 - 0.9 %

Show Material materials with Manganese of 0.3 - 0.9 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T351

EN 573-3, EN 485, EN 754

Sheet, Flat, Rod, Strip, Plate, Forging, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: poor, weathering: poor

Workability

Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O)