EN 573-3 Grade AW-2024 T3

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-2024, known for its use in aircraft industry, is an alloy that offers excellent strength. When in the annealed condition it is readily formed and has good machinability. Though it has a relatively low level of corrosion resistance, it can be machined to a high finish.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T3

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

140.0 MPa

Show Material materials with Bending Fatigue Strength of 140.0 MPa

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Bending angle 180°

4.0 °/t

Show Material materials with Bending angle 180° of 4.0 °/t

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

5.0 °/t

Show Material materials with Bending angle 180° of 5.0 °/t

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Bending angle 90°

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

5.0 °/t

Show Material materials with Bending angle 90° of 5.0 °/t

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

8.0 °/t

Show Material materials with Bending angle 90° of 8.0 °/t

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

70.0 - 74.5 GPa

Show Material materials with Elastic modulus of 70.0 - 74.5 GPa

T3

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Elongation

6.0 %

Show Material materials with Elongation of 6.0 %

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T3

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T3

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

9.0 %

Show Material materials with Elongation of 9.0 %

T3

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

10.0 %

Show Material materials with Elongation of 10.0 %

T3

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

12.0 %

Show Material materials with Elongation of 12.0 %

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

13.0 %

Show Material materials with Elongation of 13.0 %

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

14.0 %

Show Material materials with Elongation of 14.0 %

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T3

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T3

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T3

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T3

EN 573-3

Sheet

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T3

EN 573-3

Rod

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T3

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T3

EN 573-3

Tube, Sheet, Profile, Rod

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T3

EN 573-3

Rod, Tube

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T3

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T3

EN 573-3

Rod

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T3

EN 573-3

Rod, Tube

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T3

EN 573-3

Flat

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

T3

EN 573-3

Flat

Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T3

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

T3

EN 573-3

Flat

A50 Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T3

EN 573-3

Flat

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T3

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T3

EN 573-3

Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T3

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

124.0 [-]

Show Material materials with Hardness, Brinell of 124.0 [-]

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

104.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 120.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 115.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 115.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 110.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 110.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

104.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

104.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 124.0 [-]

T3

EN 573-3

Flat

20.0 °C

104.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 104.0 - 122.0 [-]

T3

EN 573-3

Flat

20.0 °C

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T3

EN 573-3

Profile, Sheet, Flat

20.0 °C

110.0 - 138.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 138.0 [-]

T3

EN 573-3

Profile

20.0 °C

110.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 120.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

110.0 - 115.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 115.0 [-]

T3

EN 573-3

Sheet, Flat

20.0 °C

110.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

110.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 124.0 [-]

T3

EN 573-3

Flat

20.0 °C

110.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 110.0 - 122.0 [-]

T3

EN 573-3

Flat

20.0 °C

115.0 [-]

Show Material materials with Hardness, Brinell of 115.0 [-]

T3

EN 573-3

Tube, Sheet, Flat

20.0 °C

115.0 - 120.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 120.0 [-]

T3

EN 573-3

Tube, Sheet, Flat

20.0 °C

115.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

115.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 124.0 [-]

T3

EN 573-3

Flat

20.0 °C

115.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 115.0 - 122.0 [-]

T3

EN 573-3

Flat

20.0 °C

120.0 [-]

Show Material materials with Hardness, Brinell of 120.0 [-]

T3

EN 573-3

Profile, Rod, Tube, Sheet, Flat

20.0 °C

120.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

120.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 124.0 [-]

T3

EN 573-3

Flat

20.0 °C

120.0 - 122.0 [-]

Show Material materials with Hardness, Brinell of 120.0 - 122.0 [-]

T3

EN 573-3

Flat

20.0 °C

122.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 122.0 - 124.0 [-]

T3

EN 573-3

Rod, Flat

20.0 °C

122.0 [-]

Show Material materials with Hardness, Brinell of 122.0 [-]

T3

EN 573-3

Rod, Flat

20.0 °C

122.0 - 123.0 [-]

Show Material materials with Hardness, Brinell of 122.0 - 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

123.0 [-]

Show Material materials with Hardness, Brinell of 123.0 [-]

T3

EN 573-3

Flat

20.0 °C

123.0 - 124.0 [-]

Show Material materials with Hardness, Brinell of 123.0 - 124.0 [-]

T3

EN 573-3

Flat

20.0 °C

124.0 [-]

Show Material materials with Hardness, Brinell of 124.0 [-]

T3

EN 573-3

Rod, Flat

20.0 °C

137.0 [-]

Show Material materials with Hardness, Brinell of 137.0 [-]

T3

EN 573-3

Tube

20.0 °C

138.0 [-]

Show Material materials with Hardness, Brinell of 138.0 [-]

T3

EN 573-3

Profile

Plane-Strain Fracture Toughnes

20.0 °C

17.5 - 41.7 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 41.7 MPa·√m

T3

EN 573-3

20.0 °C

17.5 - 33.5 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 33.5 MPa·√m

T3

EN 573-3

20.0 °C

17.5 - 18.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 17.5 - 18.0 MPa·√m

T3

EN 573-3

20.0 °C

18.0 - 41.7 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 41.7 MPa·√m

T3

EN 573-3

20.0 °C

18.0 - 33.5 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 33.5 MPa·√m

T3

EN 573-3

20.0 °C

18.0 - 26.2 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 26.2 MPa·√m

T3

EN 573-3

20.0 °C

18.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 18.0 MPa·√m

T3

EN 573-3

20.0 °C

26.2 - 41.7 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 41.7 MPa·√m

T3

EN 573-3

20.0 °C

26.2 - 33.5 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.5 MPa·√m

T3

EN 573-3

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

27.0 - 28.0 GPa

Show Material materials with Shear modulus of 27.0 - 28.0 GPa

T3

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Tensile strength

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T3

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T3

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T3

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

T3

EN 573-3

Transverse

20.0 °C

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T3

EN 573-3

Sheet

20.0 °C

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T3

EN 573-3

Sheet

20.0 °C

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T3

EN 573-3

Profile

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T3

EN 573-3

Sheet, Rod

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T3

EN 573-3

Tube, Sheet, Profile, Rod

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T3

EN 573-3

Rod

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T3

EN 573-3

Flat

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T3

EN 573-3

Flat

20.0 °C

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T3

EN 573-3

Tube, Flat, Rod

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T3

EN 573-3

Flat

Transverse

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T3

EN 573-3

Rod

Yield strength

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T3

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

280.0 MPa

Show Material materials with Yield strength of 280.0 MPa

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

300.0 MPa

Show Material materials with Yield strength of 300.0 MPa

T3

EN 573-3, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

310.0 MPa

Show Material materials with Yield strength of 310.0 MPa

T3

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

RP02

20.0 °C

140.0 MPa

Show Material materials with Yield strength of 140.0 MPa

T3

EN 573-3

RP02 Transverse

20.0 °C

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T3

EN 573-3

Sheet

RP02

20.0 °C

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T3

EN 573-3

Flat

RP02 Transverse

20.0 °C

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T3

EN 573-3

Tube, Sheet, Rod

RP02

20.0 °C

270.0 MPa

Show Material materials with Yield strength of 270.0 MPa

T3

EN 573-3

Flat

RP02 Transverse

20.0 °C

275.0 - 310.0 MPa

Show Material materials with Yield strength of 275.0 - 310.0 MPa

T3

EN 573-3

20.0 °C

280.0 MPa

Show Material materials with Yield strength of 280.0 MPa

T3

EN 573-3

Rod

RP02

20.0 °C

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T3

EN 573-3

Sheet

RP02

20.0 °C

285.0 MPa

Show Material materials with Yield strength of 285.0 MPa

T3

EN 573-3

Flat

RP02 Transverse

20.0 °C

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T3

EN 573-3

Tube, Sheet, Flat, Profile, Rod

RP02

20.0 °C

290.0 MPa

Show Material materials with Yield strength of 290.0 MPa

T3

EN 573-3

Flat

RP02 Transverse

20.0 °C

300.0 MPa

Show Material materials with Yield strength of 300.0 MPa

T3

EN 573-3

Rod

RP02

20.0 °C

310.0 MPa

Show Material materials with Yield strength of 310.0 MPa

T3

EN 573-3

Rod

RP02

20.0 °C

450.0 MPa

Show Material materials with Yield strength of 450.0 MPa

T3

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

200 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

300 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Melting point

505.0 - 640.0 °C

Show Material materials with Melting point of 505.0 - 640.0 °C

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T3

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Thermal conductivity

121.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K)

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

T3

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

17000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

18000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m

T3

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar

Electrical resistivity

3.45e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

4.76e-08 - 5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Copper

3.8 - 4.9 %

Show Material materials with Copper of 3.8 - 4.9 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T3

EN 573-3

Sheet, Flat, Profile, Rod, Tube

0.50 %

Show Material materials with Iron of 0.50 %

T3

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

1.2 - 1.8 %

Show Material materials with Magnesium of 1.2 - 1.8 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Manganese

0.3 - 0.9 %

Show Material materials with Manganese of 0.3 - 0.9 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T3

EN 573-3, EN 485, EN 754, EN 755

Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: poor, weathering: poor

Workability

Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O)