EN 573-3 Grade AW-1050A H24

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H24

EN 573-3

Flat, Foil, Plate

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

0.2 mm

Coil, Sheet, Strip

3 mm

Show Material materials with Thickness of 3 mm

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

3 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

35.0 MPa

Show Material materials with Bending Fatigue Strength of 35.0 MPa

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 180°

1 °/t

Show Material materials with Bending angle 180° of 1 °/t

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Flat, Foil, Plate

-195.0 °C

78.4 GPa

Show Material materials with Elastic modulus of 78.4 GPa

H24

EN 573-3

Flat, Foil, Plate

-85.0 °C

73.5 GPa

Show Material materials with Elastic modulus of 73.5 GPa

H24

EN 573-3

Flat, Foil, Plate

-30.0 °C

71.4 GPa

Show Material materials with Elastic modulus of 71.4 GPa

H24

EN 573-3

Flat, Foil, Plate

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3

Coil, Sheet, Strip, Flat, Foil, Plate

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H24

EN 573-3

Flat, Foil, Plate

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H24

EN 573-3

Flat, Foil, Plate

100.0 °C

68.0 - 68.6 GPa

Show Material materials with Elastic modulus of 68.0 - 68.6 GPa

H24

EN 573-3

Flat, Foil, Plate

100.0 °C

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

H24

EN 573-3

Flat, Foil, Plate

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H24

EN 573-3

Flat, Foil, Plate

150.0 °C

66.0 - 66.5 GPa

Show Material materials with Elastic modulus of 66.0 - 66.5 GPa

H24

EN 573-3

Flat, Foil, Plate

150.0 °C

66.5 GPa

Show Material materials with Elastic modulus of 66.5 GPa

H24

EN 573-3

Flat, Foil, Plate

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H24

EN 573-3

Flat, Foil, Plate

250.0 °C

56.0 - 57.0 GPa

Show Material materials with Elastic modulus of 56.0 - 57.0 GPa

H24

EN 573-3

Flat, Foil, Plate

250.0 °C

56.0 GPa

Show Material materials with Elastic modulus of 56.0 GPa

H24

EN 573-3

Flat, Foil, Plate

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H24

EN 573-3

Flat, Foil, Plate

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H24

EN 573-3

Flat, Foil, Plate

Elongation

3 %

Show Material materials with Elongation of 3 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H24

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

8.0 %

Show Material materials with Elongation of 8.0 %

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H24

EN 573-3

Plate

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H24

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H24

EN 573-3

Plate, Flat

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H24

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H24

EN 573-3

Foil

A100

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H24

EN 573-3

Foil, Plate, Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H24

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H24

EN 573-3

Foil

A100

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H24

EN 573-3

Foil, Plate, Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H24

EN 573-3

Foil

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H24

EN 573-3

Foil

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H24

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H24

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H24

EN 573-3

Plate

Hardness, Brinell

33.0 [-]

Show Material materials with Hardness, Brinell of 33.0 [-]

H24

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

33.0 [-]

Show Material materials with Hardness, Brinell of 33.0 [-]

H24

EN 573-3

Flat

Hardness, HBW

33 [-]

Show Material materials with Hardness, HBW of 33 [-]

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H24

EN 573-3

Flat, Foil, Plate

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

25.0 - 25.9 GPa

Show Material materials with Shear modulus of 25.0 - 25.9 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

25.9 - 26.5 GPa

Show Material materials with Shear modulus of 25.9 - 26.5 GPa

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H24

EN 573-3

Flat, Foil, Plate

Tensile strength

105 MPa

Show Material materials with Tensile strength of 105 MPa

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

105.0 - 145.0 MPa

Show Material materials with Tensile strength of 105.0 - 145.0 MPa

H24

EN 573-3

Flat

Transverse

20.0 °C

105.0 - 145.0 MPa

Show Material materials with Tensile strength of 105.0 - 145.0 MPa

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

Yield strength

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

75 MPa

Show Material materials with Yield strength of 75 MPa

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H24

EN 573-3

Flat

RP02 Transverse

20.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H24

EN 573-3

Foil, Plate, Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20-100°C

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H24

EN 573-3

Flat, Foil, Plate

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H24

EN 573-3

Flat, Foil, Plate

Melting point

646.0 - 657.0 °C

Show Material materials with Melting point of 646.0 - 657.0 °C

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H24

EN 573-3

Flat, Foil, Plate

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

210.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 229.0 W/(m·K)

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

220.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 - 229.0 W/(m·K)

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

229.0 W/(m·K)

Show Material materials with Thermal conductivity of 229.0 W/(m·K)

H24

EN 573-3

Flat, Foil, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 36000000.0 S/m

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34800000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34800000.0 - 36000000.0 S/m

H24

EN 573-3

Flat, Foil, Plate

Electrical resistivity

2.78e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.94e-08 Ω·m

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

20.0 °C

2.8e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 2.9e-08 Ω·m

H24

EN 573-3

Flat, Foil, Plate

20.0 °C

2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 Ω·m

H24

EN 573-3

Flat, Foil, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

Boron

0.05

Show Material materials with Boron of 0.05

H24

EN 573-3

Flat

Chromium

0.01

Show Material materials with Chromium of 0.01

H24

EN 573-3

Flat

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.05 %

Show Material materials with Copper of 0.05 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Gallium

0.03

Show Material materials with Gallium of 0.03

H24

EN 573-3

Flat

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H24

EN 573-3

Flat, Foil, Plate

0.4 %

Show Material materials with Iron of 0.4 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

0.40 %

Show Material materials with Iron of 0.40 %

H24

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H24

EN 573-3

Flat

0.05 %

Show Material materials with Magnesium of 0.05 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.05 %

Show Material materials with Magnesium of 0.05 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

H24

EN 573-3

Flat

0.05 %

Show Material materials with Manganese of 0.05 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.05 %

Show Material materials with Manganese of 0.05 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Nickel

0.03

Show Material materials with Nickel of 0.03

H24

EN 573-3

Flat

Other

0.03 %

Show Material materials with Other of 0.03 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

H24

EN 573-3

Flat

0.25 %

Show Material materials with Silicon of 0.25 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.25 %

Show Material materials with Silicon of 0.25 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H24

EN 573-3

Flat

0.05 %

Show Material materials with Titanium of 0.05 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.05 %

Show Material materials with Titanium of 0.05 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Vanadium

0.03

Show Material materials with Vanadium of 0.03

H24

EN 573-3

Flat

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H24

EN 573-3

Flat

0.07 %

Show Material materials with Zinc of 0.07 %

H24

EN 573-3, EN 485, EN 683

Flat, Foil, Plate, Strip, Sheet, Bar, Rod, Tube

0.07 %

Show Material materials with Zinc of 0.07 %

H24

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Lithography; Cable Wrapping: Electric cable wrapping; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, rotor hub, stairs; Cosmetics: Cosmetics pieces; Automotive Trim: Interior Trim, Marque Badges; Components: Heat shields, General Transportation

Brazing

Excellent

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent