EN 573-3 Grade AW-3103 H22

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Flat, Plate

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet

3.0 mm

Show Material materials with Thickness of 3.0 mm

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3.0 mm

Coil, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Flat, Plate

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

69.0 - 69.5 GPa

Show Material materials with Elastic modulus of 69.0 - 69.5 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

69.5 - 70.0 GPa

Show Material materials with Elastic modulus of 69.5 - 70.0 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Flat, Plate

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H22

EN 573-3

Foil, Flat, Plate

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H22

EN 573-3

Foil, Flat, Plate

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H22

EN 573-3

Foil, Flat, Plate

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H22

EN 573-3

Foil, Flat, Plate

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H22

EN 573-3

Foil, Flat, Plate

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H22

EN 573-3

Foil, Flat, Plate

Elongation

5.0 %

Show Material materials with Elongation of 5.0 %

H22

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H22

EN 573-3, EN 485, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6.0 - 8.0 %

Show Material materials with Elongation of 6.0 - 8.0 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

8.0 %

Show Material materials with Elongation of 8.0 %

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

10.0 %

Show Material materials with Elongation of 10.0 %

H22

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

11.0 %

Show Material materials with Elongation of 11.0 %

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H22

EN 573-3

Plate

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H22

EN 573-3

Plate

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H22

EN 573-3

Plate

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H22

EN 573-3

Foil

A100

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H22

EN 573-3

Foil, Plate

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H22

EN 573-3

Foil

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H22

EN 573-3

Foil, Plate, Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H22

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H22

EN 573-3

Foil

A100

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H22

EN 573-3

Foil, Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H22

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H22

EN 573-3

Plate

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H22

EN 573-3

Foil

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H22

EN 573-3

Foil, Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

H22

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H22

EN 573-3

Foil

A100

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H22

EN 573-3

Foil, Flat

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H22

EN 573-3

Flat

A50 Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H22

EN 573-3

Foil

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H22

EN 573-3

Foil

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H22

EN 573-3

Plate

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H22

EN 573-3

Foil

A100

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H22

EN 573-3

Foil, Flat

A50

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H22

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H22

EN 573-3

Foil

A100

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H22

EN 573-3

Foil

A50

Hardness, Brinell

36.0 [-]

Show Material materials with Hardness, Brinell of 36.0 [-]

H22

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

36.0 [-]

Show Material materials with Hardness, Brinell of 36.0 [-]

H22

EN 573-3

Flat

Hardness, HBW

36 [-]

Show Material materials with Hardness, HBW of 36 [-]

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H22

EN 573-3

Foil, Flat, Plate

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Shear modulus of 24.0 - 26.5 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

24.0 - 26.1 GPa

Show Material materials with Shear modulus of 24.0 - 26.1 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

26.1 - 26.5 GPa

Show Material materials with Shear modulus of 26.1 - 26.5 GPa

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H22

EN 573-3

Foil, Flat, Plate

Tensile strength

20.0 °C

115.0 - 155.0 MPa

Show Material materials with Tensile strength of 115.0 - 155.0 MPa

H22

EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Coil, Sheet, Flat

20.0 °C

115.0 - 175.0 MPa

Show Material materials with Tensile strength of 115.0 - 175.0 MPa

H22

EN 573-3

Plate

20.0 °C

115.0 - 195.0 MPa

Show Material materials with Tensile strength of 115.0 - 195.0 MPa

H22

EN 573-3

Plate

20.0 °C

115.0 - 155.0 MPa

Show Material materials with Tensile strength of 115.0 - 155.0 MPa

H22

EN 573-3

Flat

Transverse

20.0 °C

120.0 - 160.0 MPa

Show Material materials with Tensile strength of 120.0 - 160.0 MPa

H22

EN 573-3

Foil

20.0 °C

140.0 - 175.0 MPa

Show Material materials with Tensile strength of 140.0 - 175.0 MPa

H22

EN 573-3

Plate

20.0 °C

140.0 - 195.0 MPa

Show Material materials with Tensile strength of 140.0 - 195.0 MPa

H22

EN 573-3

Plate

Yield strength

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H22

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

75 MPa

Show Material materials with Yield strength of 75 MPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H22

EN 573-3

Flat

RP02 Transverse

20.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

H22

EN 573-3

Foil, Plate, Flat

RP02

20.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H22

EN 573-3

Foil

RP02

20.0 °C

110.0 MPa

Show Material materials with Yield strength of 110.0 MPa

H22

EN 573-3

Plate

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

0.000025 1/K

Show Material materials with Coefficient of thermal expansion of 0.000025 1/K

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20-100°C

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

892.0 - 893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 - 893.0 J/(kg·K)

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

892.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 J/(kg·K)

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H22

EN 573-3

Foil, Flat, Plate

Thermal conductivity

176 W/(m·K)

Show Material materials with Thermal conductivity of 176 W/(m·K)

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K)

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

160.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 W/(m·K)

H22

EN 573-3

Foil, Flat, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

22000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

22000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 29000000.0 S/m

H22

EN 573-3

Foil, Flat, Plate

Electrical resistivity

3.57e-08 - 4.55e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 4.55e-08 Ω·m

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 Ω·m

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

3.4e-08 - 4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.1e-08 Ω·m

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

3.4e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.5e-08 Ω·m

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 Ω·m

H22

EN 573-3

Foil, Flat, Plate

20.0 °C

4.1e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 - 4.5e-08 Ω·m

H22

EN 573-3

Foil, Flat, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H22

EN 573-3, EN 485, EN 546, EN 683

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube

0.1 %

Show Material materials with Chromium of 0.1 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H22

EN 573-3, EN 485, EN 546, EN 683

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube

0.1 %

Show Material materials with Copper of 0.1 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H22

EN 573-3

Foil, Flat, Plate

0.70 %

Show Material materials with Iron of 0.70 %

H22

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

0.7 %

Show Material materials with Iron of 0.7 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Magnesium

0.3 %

Show Material materials with Magnesium of 0.3 %

H22

EN 573-3, EN 485, EN 546, EN 683

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube

0.3 %

Show Material materials with Magnesium of 0.3 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Manganese

0.9 - 1.5 %

Show Material materials with Manganese of 0.9 - 1.5 %

H22

EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube, Coil, Sheet

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

H22

EN 573-3, EN 485, EN 546, EN 683

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube

0.5 %

Show Material materials with Silicon of 0.5 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H22

EN 573-3, EN 485, EN 546, EN 683

Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube

0.2 %

Show Material materials with Zinc of 0.2 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers

Brazing

hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12)