AA Standards Grade 2024 T361

View suppliers (122)
Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 2024, known for its use in aircraft industry, is an alloy that offers excellent strength. When in the annealed condition it is readily formed and has good machinability. Though it has a relatively low level of corrosion resistance, it can be machined to a high finish.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,WroughtAl_ElectricalResistivity.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.78 g/cm³

Show Material materials with Density of 2.78 g/cm³

T361

AA Standards, ASTM B209

3.0 g/cm³

Show Material materials with Density of 3.0 g/cm³

T361

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T361

AA Standards, ASTM B209

Elongation

8.0 %

Show Material materials with Elongation of 8.0 %

T361

AA Standards, ASTM B209

A50

9.0 %

Show Material materials with Elongation of 9.0 %

T361

AA Standards, ASTM B209

A50

9.0 %

Show Material materials with Elongation of 9.0 %

T361

AA Standards, ASTM B209

A100

12.0 %

Show Material materials with Elongation of 12.0 %

T361

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

26.0 - 27.5 GPa

Show Material materials with Shear modulus of 26.0 - 27.5 GPa

Typical for Wrought 2000 Series Aluminium

Tensile strength

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T361

AA Standards, ASTM B209

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T361

AA Standards, ASTM B209

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T361

AA Standards, ASTM B209

510.0 MPa

Show Material materials with Tensile strength of 510.0 MPa

T361

Yield strength

340.0 MPa

Show Material materials with Yield strength of 340.0 MPa

T361

AA Standards, ASTM B209

RP02

345.0 MPa

Show Material materials with Yield strength of 345.0 MPa

T361

AA Standards, ASTM B209

RP02

350.0 MPa

Show Material materials with Yield strength of 350.0 MPa

T361

AA Standards, ASTM B209

RP02

390.0 MPa

Show Material materials with Yield strength of 390.0 MPa

T361

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T361

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T361

AA Standards, ASTM B209

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

T361

AA Standards, ASTM B209

Melting point

500.0 °C

Show Material materials with Melting point of 500.0 °C

T361

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T361

AA Standards, ASTM B209

Specific heat capacity

870.0 J/(kg·K)

Show Material materials with Specific heat capacity of 870.0 J/(kg·K)

T361

Thermal conductivity

120.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 W/(m·K)

T361

121.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K)

T361

AA Standards, ASTM B209

Electrical

PropertyValueConditionRelated StandardsComment

Electrical conductivity

17000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m

T361

AA Standards, ASTM B209

17000000 S/m

Show Material materials with Electrical conductivity of 17000000 S/m

T361

Typical/derived value

Electrical resistivity

3.45e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m

T361

AA Standards, ASTM B209

5.8999999999999986e-08 Ω·m

Show Material materials with Electrical resistivity of 5.8999999999999986e-08 Ω·m

T361

Typical value

Specific Electrical conductivity

30.0 % IACS

Show Material materials with Specific Electrical conductivity of 30.0 % IACS

T361

Typical value

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

90.7 - 94.7 %

Show Material materials with Aluminium of 90.7 - 94.7 %

T361

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T361

AA Standards, ASTM B209

Copper

3.8 - 4.9 %

Show Material materials with Copper of 3.8 - 4.9 %

T361

AA Standards, ASTM B209

Iron

0.50 %

Show Material materials with Iron of 0.50 %

T361

AA Standards, ASTM B209

0.5 %

Show Material materials with Iron of 0.5 %

T361

Magnesium

1.2 - 1.8 %

Show Material materials with Magnesium of 1.2 - 1.8 %

T361

AA Standards, ASTM B209

Manganese

0.3 - 0.9 %

Show Material materials with Manganese of 0.3 - 0.9 %

T361

AA Standards, ASTM B209

Other

0.15 %

Show Material materials with Other of 0.15 %

T361

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

T361

AA Standards, ASTM B209

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T361

AA Standards, ASTM B209

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T361

AA Standards, ASTM B209

Zirconium

0.2 %

Show Material materials with Zirconium of 0.2 %

T361

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T4,T3, T351, T3510, T3511), d (T6, T861, T81, T851, T8510, T8511), general: sufficient, in principle it should be protected

General machinability

General: poor (O), good to acceptable

Workability

general (condition): poor(T4, T3, T351, T3510, T3511, T6), not suitable (T361, T861, T81, T851, T8510, T8511)