This material data has been provided by AluKey,MakeItFrom.com,WroughtAl_ElectricalResistivity.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.84 - 3.1 g/cm³

Show Material materials with Density of 2.84 - 3.1 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

73 - 74 GPa

Show Material materials with Elastic modulus of 73 - 74 GPa

Elongation

23.0 °C

14 %

Show Material materials with Elongation of 14 %

Elongation A100

23.0 °C

12 %

Show Material materials with Elongation A100 of 12 %

Elongation A50

23.0 °C

8 - 17 %

Show Material materials with Elongation A50 of 8 - 17 %

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

23.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

23.0 °C

26 - 27.5 GPa

Show Material materials with Shear modulus of 26 - 27.5 GPa

Typical for Wrought 2000 Series Aluminium

Tensile strength

23.0 °C

290 - 360 MPa

Show Material materials with Tensile strength of 290 - 360 MPa

Yield strength

23.0 °C

230 MPa

Show Material materials with Yield strength of 230 MPa

Yield strength Rp0.2

23.0 °C

180 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 180 - 250 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

20.0 °C

2.23E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.23E-5 1/K

23.0 °C

2.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.2E-5 1/K

100.0 °C

2.23E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.23E-5 1/K

Melting point

540 - 645 °C

Show Material materials with Melting point of 540 - 645 °C

Specific heat capacity

23.0 °C

860 J/(kg·K)

Show Material materials with Specific heat capacity of 860 J/(kg·K)

Thermal conductivity

23.0 °C

110 - 172 W/(m·K)

Show Material materials with Thermal conductivity of 110 - 172 W/(m·K)

Electrical

PropertyTemperatureValueComment

Electrical conductivity

23.0 °C

1.60E+7 - 2.60E+7 S/m

Show Material materials with Electrical conductivity of 1.60E+7 - 2.60E+7 S/m

Typical value

Electrical resistivity

23.0 °C

3.85E-8 - 6.25E-8 Ω·m

Show Material materials with Electrical resistivity of 3.85E-8 - 6.25E-8 Ω·m

Typical value

Specific Electrical conductivity

28 % IACS

Show Material materials with Specific Electrical conductivity of 28 % IACS

Typical/Derived value

Chemical properties

PropertyValueComment

Aluminium

91.5 - 93.8 %

Show Material materials with Aluminium of 91.5 - 93.8 %

Copper

5.8 - 6.8 %

Show Material materials with Copper of 5.8 - 6.8 %

Iron

0 - 0.3 %

Show Material materials with Iron of 0 - 0.3 %

Magnesium

0 - 0.02 %

Show Material materials with Magnesium of 0 - 0.02 %

Manganese

0.2 - 0.4 %

Show Material materials with Manganese of 0.2 - 0.4 %

Other

0 - 0.15 %

Show Material materials with Other of 0 - 0.15 %

each 0.05, total 0.15, Rest Al

Silicon

0 - 0.2 %

Show Material materials with Silicon of 0 - 0.2 %

Titanium

0.02 - 0.1 %

Show Material materials with Titanium of 0.02 - 0.1 %

Vanadium

0.05 - 0.15 %

Show Material materials with Vanadium of 0.05 - 0.15 %

Zinc

0 - 0.1 %

Show Material materials with Zinc of 0 - 0.1 %

Zirconium

0.1 - 0.25 %

Show Material materials with Zirconium of 0.1 - 0.25 %

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected

General machinability

General: good to acceptable

Workability

general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87)