AA Standards Grade 2219 T6

Want to keep this datasheet? Save it now in your required format

Description

Aluminum Alloy AA 2219, an age-hardenable alloy is produced with a copper additive. It is well-known for its excellent structural strength and it’s used for numerous high temperature applications. It is a suitable alloy for many metalworking processes including machining, forming, heat treatment, cold working, and more.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,WroughtAl_ElectricalResistivity.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.84 g/cm³

Show Material materials with Density of 2.84 g/cm³

T6

AA Standards, ASTM B247, ASTM B316

3.1 g/cm³

Show Material materials with Density of 3.1 g/cm³

T6

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T6

AA Standards, ASTM B247, ASTM B316

74.0 GPa

Show Material materials with Elastic modulus of 74.0 GPa

T6

Elongation

6.0 %

Show Material materials with Elongation of 6.0 %

T6

AA Standards, ASTM B247

A50

2.0 %

Show Material materials with Elongation of 2.0 %

T6

AA Standards, ASTM B247

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T6

AA Standards, ASTM B247

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T6

AA Standards, ASTM B247

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T6

AA Standards, ASTM B247, ASTM B316

A100

1.0 %

Show Material materials with Elongation of 1.0 %

T6

AA Standards, ASTM B247

A100

3.0 %

Show Material materials with Elongation of 3.0 %

T6

AA Standards, ASTM B247

A100

7.0 %

Show Material materials with Elongation of 7.0 %

T6

AA Standards, ASTM B247

A100

5.5 %

Show Material materials with Elongation of 5.5 %

T6

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

26.0 - 27.5 GPa

Show Material materials with Shear modulus of 26.0 - 27.5 GPa

Typical for Wrought 2000 Series Aluminium

Tensile strength

385.0 MPa

Show Material materials with Tensile strength of 385.0 MPa

T6

AA Standards, ASTM B247

365.0 MPa

Show Material materials with Tensile strength of 365.0 MPa

T6

AA Standards, ASTM B247

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T6

AA Standards, ASTM B247

380.0 MPa

Show Material materials with Tensile strength of 380.0 MPa

T6

AA Standards, ASTM B247, ASTM B316

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

Yield strength

275.0 MPa

Show Material materials with Yield strength of 275.0 MPa

T6

AA Standards, ASTM B247

RP02

240.0 MPa

Show Material materials with Yield strength of 240.0 MPa

T6

AA Standards, ASTM B247, ASTM B316

RP02

250.0 MPa

Show Material materials with Yield strength of 250.0 MPa

T6

AA Standards, ASTM B247

RP02

255.0 MPa

Show Material materials with Yield strength of 255.0 MPa

T6

AA Standards, ASTM B247

RP02

260.0 MPa

Show Material materials with Yield strength of 260.0 MPa

T6

AA Standards, ASTM B247

RP02

280.0 MPa

Show Material materials with Yield strength of 280.0 MPa

T6

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.2e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K

T6

100 °C, 20 °C

2.23e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.23e-05 1/K

T6

AA Standards, ASTM B247, ASTM B316

Melting point

545.0 - 645.0 °C

Show Material materials with Melting point of 545.0 - 645.0 °C

T6

AA Standards, ASTM B247, ASTM B316

540.0 °C

Show Material materials with Melting point of 540.0 °C

T6

Specific heat capacity

860.0 J/(kg·K)

Show Material materials with Specific heat capacity of 860.0 J/(kg·K)

T6

Thermal conductivity

113.0 - 172.0 W/(m·K)

Show Material materials with Thermal conductivity of 113.0 - 172.0 W/(m·K)

T6

AA Standards, ASTM B247, ASTM B316

120.0 W/(m·K)

Show Material materials with Thermal conductivity of 120.0 W/(m·K)

T6

Electrical

PropertyValueConditionRelated StandardsComment

Electrical conductivity

16000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 26000000.0 S/m

T6

AA Standards, ASTM B247, ASTM B316

17000000 S/m

Show Material materials with Electrical conductivity of 17000000 S/m

T6

Typical value

Electrical resistivity

3.85e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 6.25e-08 Ω·m

T6

AA Standards, ASTM B247, ASTM B316

5.8999999999999986e-08 Ω·m

Show Material materials with Electrical resistivity of 5.8999999999999986e-08 Ω·m

T6

Typical value

Specific Electrical conductivity

29.0 % IACS

Show Material materials with Specific Electrical conductivity of 29.0 % IACS

T6

Typical/Derived value

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

91.5 - 93.8 %

Show Material materials with Aluminium of 91.5 - 93.8 %

T6

Copper

5.8 - 6.8 %

Show Material materials with Copper of 5.8 - 6.8 %

T6

AA Standards, ASTM B247, ASTM B316

Iron

0.30 %

Show Material materials with Iron of 0.30 %

T6

AA Standards, ASTM B247, ASTM B316

0.3 %

Show Material materials with Iron of 0.3 %

T6

Magnesium

0.02 %

Show Material materials with Magnesium of 0.02 %

T6

AA Standards, ASTM B247, ASTM B316

Manganese

0.2 - 0.4 %

Show Material materials with Manganese of 0.2 - 0.4 %

T6

AA Standards, ASTM B247, ASTM B316

Other

0.15 %

Show Material materials with Other of 0.15 %

T6

Silicon

0.2 %

Show Material materials with Silicon of 0.2 %

T6

AA Standards, ASTM B247, ASTM B316

Titanium

0.02 - 0.1 %

Show Material materials with Titanium of 0.02 - 0.1 %

T6

AA Standards, ASTM B247, ASTM B316

Vanadium

0.05 - 0.15 %

Show Material materials with Vanadium of 0.05 - 0.15 %

T6

AA Standards, ASTM B247, ASTM B316

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

T6

AA Standards, ASTM B247, ASTM B316

Zirconium

0.1 - 0.25 %

Show Material materials with Zirconium of 0.1 - 0.25 %

T6

AA Standards, ASTM B247, ASTM B316

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected

General machinability

General: good to acceptable

Workability

general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87)