AA Standards Grade 3003 H24

View suppliers (176)
Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 3003 is a popular alloy that offers customers very good atmospheric corrosion resistance and moderate strength. Aluminum 3003 offers good machinability for aluminum alloys, though it is not heat treatable. Unlike other aluminum alloys, AA 3003 is weldable by conventional welding methods. It also takes cold and hot working well and has generally better mechanical properties when compared to 1000 series aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by Gränges,AluKey,MakeItFrom.com.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H24

AA Standards, ASTM B209

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

H24

Dimension

PropertyValueConditionShape

Dimensions

<p>Standard process capabilities:</p> <p>Width: 10-1400mm</p> <p>Thickness 0.050-3.18mm</p>

H24

Coil

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H24

AA Standards, ASTM B209

Elongation

0.5 %

Show Material materials with Elongation of 0.5 %

H24

Coil

Min., A50

1.0 %

Show Material materials with Elongation of 1.0 %

H24

AA Standards, ASTM B209

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H24

AA Standards, ASTM B209

A50

2.9 %

Show Material materials with Elongation of 2.9 %

H24

3.0 %

Show Material materials with Elongation of 3.0 %

H24

AA Standards, ASTM B209

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H24

AA Standards, ASTM B209

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H24

AA Standards, ASTM B209

A100

8.0 %

Show Material materials with Elongation of 8.0 %

H24

AA Standards, ASTM B209

A50

20.0 %

Show Material materials with Elongation of 20.0 %

H24

Coil

Min., A50

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

25.0 - 26.0 GPa

Show Material materials with Shear modulus of 25.0 - 26.0 GPa

Typical for Wrought 3000 Series Aluminium

Tensile strength

110 MPa

Show Material materials with Tensile strength of 110 MPa

H24

Coil

140.0 - 180.0 MPa

Show Material materials with Tensile strength of 140.0 - 180.0 MPa

H24

AA Standards, ASTM B209

160.0 - 220.0 MPa

Show Material materials with Tensile strength of 160.0 - 220.0 MPa

H24

Coil

160 MPa

Show Material materials with Tensile strength of 160 MPa

H24

Yield strength

50.0 MPa

Show Material materials with Yield strength of 50.0 MPa

H24

Coil

RP02

115.0 MPa

Show Material materials with Yield strength of 115.0 MPa

H24

AA Standards, ASTM B209

RP02

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H24

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H24

Coil

RP02

Thermal

PropertyTemperatureValueConditionShapeRelated StandardsComment

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

H24

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H24

Coil

for 20-100°C

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H24

AA Standards, ASTM B209

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H24

AA Standards, ASTM B209

Melting point

605 °C

Show Material materials with Melting point of 605 °C

H24

Coil

Mean

607 °C

Show Material materials with Melting point of 607 °C

H24

Coil

Mean

618 °C

Show Material materials with Melting point of 618 °C

H24

Coil

Mean

623 °C

Show Material materials with Melting point of 623 °C

H24

Coil

Mean

640 °C

Show Material materials with Melting point of 640 °C

H24

Coil

Mean

640.0 °C

Show Material materials with Melting point of 640.0 °C

H24

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

H24

AA Standards, ASTM B209

642 °C

Show Material materials with Melting point of 642 °C

H24

Coil

Mean

Specific heat capacity

889.0 J/(kg·K)

Show Material materials with Specific heat capacity of 889.0 J/(kg·K)

H24

Coil

890.0 J/(kg·K)

Show Material materials with Specific heat capacity of 890.0 J/(kg·K)

H24

Thermal conductivity

159.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 159.0 - 193.0 W/(m·K)

H24

AA Standards, ASTM B209

160 W/(m·K)

Show Material materials with Thermal conductivity of 160 W/(m·K)

H24

Coil

After brazing, calculated from electric resistivity data measured at room temperature

180.0 W/(m·K)

Show Material materials with Thermal conductivity of 180.0 W/(m·K)

H24

Electrical

PropertyValueConditionShapeRelated StandardsComment

Corrosion potential

-720.0 mV

Show Material materials with Corrosion potential of -720.0 mV

H24

Coil

-705.0 mV

Show Material materials with Corrosion potential of -705.0 mV

H24

Coil

-690.0 mV

Show Material materials with Corrosion potential of -690.0 mV

H24

Coil

Electrical conductivity

24000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 29000000.0 S/m

H24

AA Standards, ASTM B209

Electrical resistivity

3.4e-08 - 4.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.3e-08 Ω·m

H24

Coil

Changes depending on temper

3.45e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 4.17e-08 Ω·m

H24

AA Standards, ASTM B209

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

96.8 - 99.0 %

Show Material materials with Aluminium of 96.8 - 99.0 %

H24

Copper

0.05 - 0.2 %

Show Material materials with Copper of 0.05 - 0.2 %

H24

AA Standards, ASTM B209

0.4 - 0.7 %

Show Material materials with Copper of 0.4 - 0.7 %

H24

Coil

Iron

0.1 - 0.5 %

Show Material materials with Iron of 0.1 - 0.5 %

H24

Coil

0.7 %

Show Material materials with Iron of 0.7 %

H24

0.70 %

Show Material materials with Iron of 0.70 %

H24

AA Standards, ASTM B209

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H24

AA Standards, ASTM B209

1.2 - 1.6 %

Show Material materials with Manganese of 1.2 - 1.6 %

H24

Coil

Other

0.15 %

Show Material materials with Other of 0.15 %

H24

Silicon

0.4 - 0.8 %

Show Material materials with Silicon of 0.4 - 0.8 %

H24

Coil

0.6 %

Show Material materials with Silicon of 0.6 %

H24

AA Standards, ASTM B209

Titanium

0.1 - 0.2 %

Show Material materials with Titanium of 0.1 - 0.2 %

H24

Coil

Zinc

0.0 - 0.1 %

Show Material materials with Zinc of 0.0 - 0.1 %

H24

Coil

0.05 %

Show Material materials with Zinc of 0.05 %

H24

Coil

0.10 %

Show Material materials with Zinc of 0.10 %

H24

Coil

0.1 %

Show Material materials with Zinc of 0.1 %

H24

Coil

0.1 %

Show Material materials with Zinc of 0.1 %

H24

AA Standards, ASTM B209

0.2 %

Show Material materials with Zinc of 0.2 %

H24

Coil

Zirconium

0.0 - 0.1 %

Show Material materials with Zirconium of 0.0 - 0.1 %

H24

Coil

Technological properties

Property
Application areas

Automotive, Heat Exchangers

Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12), poor (H14, H16, H25)

Heat Treatment

Age Hardenable

Processing history

Temper: H24

Workability

general (condition): good (O, H12), acceptable (H14, H25), poor(H16, H18)