General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 69 GPa Show Material materials with Elastic modulus of 69 GPa |
Elongation | 20.0 °C | 1.2 % Show Material materials with Elongation of 1.2 % |
Tensile strength | 20.0 °C | 310 MPa Show Material materials with Tensile strength of 310 MPa |
Yield strength | 20.0 °C | 280 MPa Show Material materials with Yield strength of 280 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 20.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K |
Melting point | 630 °C Show Material materials with Melting point of 630 °C | |
Specific heat capacity | 20.0 °C | 890 J/(kg·K) Show Material materials with Specific heat capacity of 890 J/(kg·K) |
Thermal conductivity | 20.0 °C | 160 W/(m·K) Show Material materials with Thermal conductivity of 160 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 95.6 - 98.2 % Show Material materials with Aluminium of 95.6 - 98.2 % |
Copper | 0.25 % Show Material materials with Copper of 0.25 % |
Iron | 0.7 % Show Material materials with Iron of 0.7 % |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % |
Manganese | 1 - 1.5 % Show Material materials with Manganese of 1 - 1.5 % |
Other | 0.15 % Show Material materials with Other of 0.15 % |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % |