AA Standards Grade 3105 H16

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,ASM Handbook Volume 2 Properties and Selection: Nonferrous Alloys and Special-Purpose Materials.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H16

AA Standards, ASTM B209

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

H16

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H16

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H16

AA Standards, ASTM B209

69 GPa

Show Material materials with Elastic modulus of 69 GPa

H16

Elongation

4.0 %

Show Material materials with Elongation of 4.0 %

H16

AA Standards

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H16

AA Standards, ASTM B209

A50

1.0 %

Show Material materials with Elongation of 1.0 %

H16

AA Standards, ASTM B209

A50

2.6 %

Show Material materials with Elongation of 2.6 %

H16

4 %

Show Material materials with Elongation of 4 %

H16

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

H16

Shear strength

110.0 MPa

Show Material materials with Shear strength of 110.0 MPa

H16

Tensile strength

195.0 MPa

Show Material materials with Tensile strength of 195.0 MPa

H16

AA Standards

170.0 - 220.0 MPa

Show Material materials with Tensile strength of 170.0 - 220.0 MPa

H16

AA Standards, ASTM B209

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H16

195 MPa

Show Material materials with Tensile strength of 195 MPa

H16

Yield strength

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H16

AA Standards

RP02

145.0 MPa

Show Material materials with Yield strength of 145.0 MPa

H16

AA Standards, ASTM B209

RP02

170 MPa

Show Material materials with Yield strength of 170 MPa

H16

RP02

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H16

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

H16

100 °C, 20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H16

AA Standards, ASTM B209

Melting point

635.0 - 655.0 °C

Show Material materials with Melting point of 635.0 - 655.0 °C

H16

AA Standards, ASTM B209

640.0 °C

Show Material materials with Melting point of 640.0 °C

H16

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H16

Thermal conductivity

172 W/(m·K)

Show Material materials with Thermal conductivity of 172 W/(m·K)

H16

AA Standards, ASTM B209

170.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 W/(m·K)

H16

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

26000000.0 S/m

Show Material materials with Electrical conductivity of 26000000.0 S/m

H16

AA Standards, ASTM B209

Electrical resistivity

3.85e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 Ω·m

H16

AA Standards, ASTM B209

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

96.0 - 99.5 %

Show Material materials with Aluminium of 96.0 - 99.5 %

H16

Chromium

0.2 %

Show Material materials with Chromium of 0.2 %

H16

AA Standards, ASTM B209

Copper

0.3 %

Show Material materials with Copper of 0.3 %

H16

AA Standards, ASTM B209

Iron

0.70 %

Show Material materials with Iron of 0.70 %

H16

AA Standards, ASTM B209

0.7 %

Show Material materials with Iron of 0.7 %

H16

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

H16

AA Standards, ASTM B209

Manganese

0.3 - 0.8 %

Show Material materials with Manganese of 0.3 - 0.8 %

H16

AA Standards, ASTM B209

Other

0.15 %

Show Material materials with Other of 0.15 %

H16

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

H16

AA Standards, ASTM B209

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H16

AA Standards, ASTM B209

Zinc

0.4 %

Show Material materials with Zinc of 0.4 %

H16

AA Standards, ASTM B209

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12), poor (H14, H25, H16, H18)

Workability

general (condition): good (O), acceptable (H12, H14, H25), poor(H16, H18)