General
Property | Value | Temperature |
---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 69 GPa Show Material materials with Elastic modulus of 69 GPa at 23.0 °C | 23.0 °C | |
Elongation | 4 % Show Material materials with Elongation of 4 % at 23.0 °C | 23.0 °C | |
Elongation A100 | 9 % Show Material materials with Elongation A100 of 9 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 3 - 10 % Show Material materials with Elongation A50 of 3 - 10 % at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 5000 Series Aluminium |
Tensile strength | 120 - 160 MPa Show Material materials with Tensile strength of 120 - 160 MPa at 23.0 °C | 23.0 °C | |
Yield strength | 96 MPa Show Material materials with Yield strength of 96 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 85 MPa Show Material materials with Yield strength Rp0.2 of 85 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 20.0 °C | 20.0 °C | |
2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K at 23.0 °C | 23.0 °C | ||
2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K at 100.0 °C | 100.0 °C | ||
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 630 - 655 °C Show Material materials with Melting point of 630 - 655 °C | ||
Specific heat capacity | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) at 23.0 °C | 23.0 °C | |
Thermal conductivity | 200 - 201 W/(m·K) Show Material materials with Thermal conductivity of 200 - 201 W/(m·K) at 23.0 °C | 23.0 °C |
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 3.00E+7 S/m Show Material materials with Electrical conductivity of 3.00E+7 S/m at 23.0 °C | 23.0 °C |
Electrical resistivity | 3.33E-8 Ω·m Show Material materials with Electrical resistivity of 3.33E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Aluminium | 97 - 99.5 % | |
Chromium | 0 - 0.1 % | |
Copper | 0 - 0.2 % | |
Iron | 0 - 0.7 % | |
Magnesium | 0.5 - 1.1 % | |
Manganese | 0 - 0.2 % | |
Other | 0 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0 - 0.3 % | |
Zinc | 0 - 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12, H32), poor (H14, H34, H16, H18, H36, H38) | |
Workability | general (condition): good (O, H12, H32), acceptable (H14, H34), poor(H16, H18, H36, H38) |