General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 69 GPa Show Material materials with Elastic modulus of 69 GPa | |
Elongation | 23.0 °C | 4.1 - 6 % Show Material materials with Elongation of 4.1 - 6 % | |
Elongation A50 | 23.0 °C | 1 - 6 % Show Material materials with Elongation A50 of 1 - 6 % | |
Hardness, Brinell | 23.0 °C | 46 [-] Show Material materials with Hardness, Brinell of 46 [-] | 500 kg load, 10 mm ball |
Plane-Strain Fracture Toughnes | 23.0 °C | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m | Typical for Wrought 5000 Series Aluminium |
Poisson's ratio | 23.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium |
Shear modulus | 23.0 °C | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | |
Shear strength | 23.0 °C | 103 MPa Show Material materials with Shear strength of 103 MPa | |
Tensile strength | 23.0 °C | 160 - 200 MPa Show Material materials with Tensile strength of 160 - 200 MPa | |
Yield strength | 23.0 °C | 150 MPa Show Material materials with Yield strength of 150 MPa | |
Yield strength Rp0.2 | 23.0 °C | 125 - 165 MPa Show Material materials with Yield strength Rp0.2 of 125 - 165 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K | |
23.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K | ||
100.0 °C | 2.38E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K | ||
Max service temperature | 150 °C Show Material materials with Max service temperature of 150 °C | Typical for Wrought 5000 Series Aluminium | |
Melting point | 630 - 655 °C Show Material materials with Melting point of 630 - 655 °C | ||
Specific heat capacity | 23.0 °C | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 200 - 201 W/(m·K) Show Material materials with Thermal conductivity of 200 - 201 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 23.0 °C | 3.00E+7 S/m Show Material materials with Electrical conductivity of 3.00E+7 S/m |
Electrical resistivity | 23.0 °C | 3.33E-8 Ω·m Show Material materials with Electrical resistivity of 3.33E-8 Ω·m |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 97 - 99.5 % Show Material materials with Aluminium of 97 - 99.5 % | |
Chromium | 0 - 0.1 % Show Material materials with Chromium of 0 - 0.1 % | |
Copper | 0 - 0.2 % Show Material materials with Copper of 0 - 0.2 % | |
Iron | 0 - 0.7 % Show Material materials with Iron of 0 - 0.7 % | |
Magnesium | 0.5 - 1.1 % Show Material materials with Magnesium of 0.5 - 1.1 % | |
Manganese | 0 - 0.2 % Show Material materials with Manganese of 0 - 0.2 % | |
Other | 0 - 0.15 % Show Material materials with Other of 0 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0 - 0.3 % Show Material materials with Silicon of 0 - 0.3 % | |
Zinc | 0 - 0.25 % Show Material materials with Zinc of 0 - 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12, H32), poor (H14, H34, H16, H18, H36, H38) | |
Workability | general (condition): good (O, H12, H32), acceptable (H14, H34), poor(H16, H18, H36, H38) |