AA Standards Grade 5052 H112

Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 5052 is a non-heat treatable alloy with excellent finishing qualities. AA 5052 offers better corrosion resistance than most aluminum alloys, especially to salt water and marine atmospheres. This alloy can be readily welded using most common techniques and is in fact offers some of the best welding characteristics of all aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

H112

AA Standards, ASTM B209, ASTM B547

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H112

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

AA Standards, ASTM B209, ASTM B547

Elongation

14.0 %

Show Material materials with Elongation of 14.0 %

H112

AA Standards, ASTM B209

A100

10.0 %

Show Material materials with Elongation of 10.0 %

H112

AA Standards, ASTM B209

A100

7.0 %

Show Material materials with Elongation of 7.0 %

H112

AA Standards, ASTM B209, ASTM B547

A50

11.0 %

Show Material materials with Elongation of 11.0 %

H112

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 5000 Series Aluminium

Tensile strength

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H112

AA Standards, ASTM B209

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H112

AA Standards, ASTM B209, ASTM B547

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

Yield strength

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

H112

AA Standards, ASTM B209

RP02

110.0 MPa

Show Material materials with Yield strength of 110.0 MPa

H112

AA Standards, ASTM B209, ASTM B547

RP02

91.0 MPa

Show Material materials with Yield strength of 91.0 MPa

H112

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

H112

100 °C, 20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H112

AA Standards, ASTM B209, ASTM B547

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

605.0 - 650.0 °C

Show Material materials with Melting point of 605.0 - 650.0 °C

H112

AA Standards, ASTM B209, ASTM B547

610.0 °C

Show Material materials with Melting point of 610.0 °C

H112

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H112

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H112

AA Standards, ASTM B209, ASTM B547

140.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 W/(m·K)

H112

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

20000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 S/m

H112

AA Standards, ASTM B209, ASTM B547

Electrical resistivity

5e-08 Ω·m

Show Material materials with Electrical resistivity of 5e-08 Ω·m

H112

AA Standards, ASTM B209, ASTM B547

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

95.8 - 97.7 %

Show Material materials with Aluminium of 95.8 - 97.7 %

H112

Chromium

0.15 - 0.35 %

Show Material materials with Chromium of 0.15 - 0.35 %

H112

AA Standards, ASTM B209, ASTM B547

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H112

AA Standards, ASTM B209, ASTM B547

Iron

0.40 %

Show Material materials with Iron of 0.40 %

H112

AA Standards, ASTM B209, ASTM B547

0.4 %

Show Material materials with Iron of 0.4 %

H112

Magnesium

2.2 - 2.8 %

Show Material materials with Magnesium of 2.2 - 2.8 %

H112

AA Standards, ASTM B209, ASTM B547

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

H112

AA Standards, ASTM B209, ASTM B547

Other

0.15 %

Show Material materials with Other of 0.15 %

H112

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H112

AA Standards, ASTM B209, ASTM B547

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H112

AA Standards, ASTM B209, ASTM B547

Technological properties

Property
Brazing

general: limited brazing

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: poor (O, H32), sufficient (H34, H36, H38)

Workability

general (condition): good (O), acceptable (H32, H34), poor(H36, H38)