See where AA Standards Grade 5052 H24 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.
Density
ρ2.68 - 2.7 g/cm³ at 20 °C
Dimensions
Dicke
Coefficient of thermal expansion
α2.38E-5 - 2.4E-5 1/K at 20 °C
Max service temperature
Tmax150 °C
Typical for Wrought 5000 Series Aluminium
Melting point
Tm605 - 650 °C
Specific heat capacity
cp900 J/(kg·K) at 20 °C
Thermal conductivity
λ138 - 140 W/(m·K) at 20 °C
Electrical conductivity
σel2.00E+7 - 2.03E+8 S/m at 20 °C
Electrical resistivity
ρel5E-8 Ω·m at 20 °C
Element
Weight %
Comment
95.8 - 97.7 %
2.2 - 2.8 %
0.15 - 0.35 %
0 - 0.1 %
0 - 0.4 %
Brazing
general: limited brazing
Corrosion properties
Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere
General machinability
General: poor (O, H32), sufficient (H34, H36, H38)
Workability
general (condition): good (O), acceptable (H32, H34), poor(H36, H38)
This material data has been provided by MakeItFrom.com,AluKey.