Description

Aluminium alloy 5052 in H32 temper has very good corrosion resistance to seawater and marine and industrial atmosphere. It also has very good weld abilityand good cold formability. It is a medium to high strength alloy with a strength slightly higher than 5251 and a medium to high fatigue strength.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,ASM Handbook Volume 2 Properties and Selection: Nonferrous Alloys and Special-Purpose Materials,Righton Blackburns.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.68 - 2.7 g/cm³

Show Material materials with Density of 2.68 - 2.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Bending Fatigue Strength

23.0 °C

115 MPa

Show Material materials with Bending Fatigue Strength of 115 MPa

Elastic modulus

23.0 °C

70 GPa

Show Material materials with Elastic modulus of 70 GPa

Elongation

23.0 °C

12 - 15 %

Show Material materials with Elongation of 12 - 15 %

Elongation A100

23.0 °C

10 - 16 %

Show Material materials with Elongation A100 of 10 - 16 %

Elongation A50

23.0 °C

4 - 12 %

Show Material materials with Elongation A50 of 4 - 12 %

Fatigue strength

23.0 °C

115 MPa

Show Material materials with Fatigue strength of 115 MPa

for 5x10⁸ cycles

Hardness, Brinell

23.0 °C

60 - 61 [-]

Show Material materials with Hardness, Brinell of 60 - 61 [-]

500 kg load, 10 mm ball

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

23.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

23.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

Shear strength

23.0 °C

140 MPa

Show Material materials with Shear strength of 140 MPa

Tensile strength

23.0 °C

210 - 265 MPa

Show Material materials with Tensile strength of 210 - 265 MPa

Yield strength

23.0 °C

180 MPa

Show Material materials with Yield strength of 180 MPa

Yield strength Rp0.2

23.0 °C

130 - 195 MPa

Show Material materials with Yield strength Rp0.2 of 130 - 195 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

2.38E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K

23.0 °C

2.37E-5 - 2.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.37E-5 - 2.4E-5 1/K

100.0 °C

2.38E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.38E-5 1/K

Max service temperature

150 °C

Show Material materials with Max service temperature of 150 °C

Typical for Wrought 5000 Series Aluminium

Melting point

605 - 650 °C

Show Material materials with Melting point of 605 - 650 °C

Specific heat capacity

23.0 °C

900 J/(kg·K)

Show Material materials with Specific heat capacity of 900 J/(kg·K)

Thermal conductivity

23.0 °C

138 - 140 W/(m·K)

Show Material materials with Thermal conductivity of 138 - 140 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

23.0 °C

2.00E+7 S/m

Show Material materials with Electrical conductivity of 2.00E+7 S/m

Electrical resistivity

23.0 °C

4.95E-8 - 5E-8 Ω·m

Show Material materials with Electrical resistivity of 4.95E-8 - 5E-8 Ω·m

Chemical properties

PropertyValueComment

Aluminium

95.8 - 97.7 %

Show Material materials with Aluminium of 95.8 - 97.7 %

Balance

Chromium

0.15 - 0.35 %

Show Material materials with Chromium of 0.15 - 0.35 %

Copper

0 - 0.1 %

Show Material materials with Copper of 0 - 0.1 %

Iron

0 - 0.4 %

Show Material materials with Iron of 0 - 0.4 %

Magnesium

2.2 - 2.8 %

Show Material materials with Magnesium of 2.2 - 2.8 %

Manganese

0 - 0.1 %

Show Material materials with Manganese of 0 - 0.1 %

Other

0 - 0.15 %

Show Material materials with Other of 0 - 0.15 %

each 0.05, total 0.15, Rest Al,Total

Silicon

0 - 0.25 %

Show Material materials with Silicon of 0 - 0.25 %

Zinc

0 - 0.1 %

Show Material materials with Zinc of 0 - 0.1 %

Technological properties

Property
Application areas

Treadplate, Boilermaking, Containers, Nameplates, Road Signs, Architectural Paneling, Welded Tubes, Chemical Industry, Irrigation, Desalination units, Pressure Vessels, Rivets,Factory flooring, conveyors, indoor and outdoor walkways, steps, stairways, gantries, bridges, cranes, commercial vehicles

Brazing

general: limited brazing

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: poor (O, H32), sufficient (H34, H36, H38)

Soldering general

Not recommended

Welding

Gas: Good; Arc: Very Good; Resistance: Very Good

Workability

general (condition): good (O), acceptable (H32, H34), poor(H36, H38)