General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 70 GPa Show Material materials with Elastic modulus of 70 GPa |
Elongation | 20.0 °C | 12 % Show Material materials with Elongation of 12 % |
Elongation A50 | 20.0 °C | 4 - 12 % Show Material materials with Elongation A50 of 4 - 12 % |
Hardness, Brinell | 20.0 °C | 60 [-] Show Material materials with Hardness, Brinell of 60 [-] |
Tensile strength | 20.0 °C | 215 - 240 MPa Show Material materials with Tensile strength of 215 - 240 MPa |
Yield strength | 20.0 °C | 180 MPa Show Material materials with Yield strength of 180 MPa |
Yield strength Rp0.2 | 20.0 °C | 160 - 195 MPa Show Material materials with Yield strength Rp0.2 of 160 - 195 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 20.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K |
Melting point | 610 °C Show Material materials with Melting point of 610 °C | |
Specific heat capacity | 20.0 °C | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) |
Thermal conductivity | 20.0 °C | 140 W/(m·K) Show Material materials with Thermal conductivity of 140 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 95.8 - 97.7 % Show Material materials with Aluminium of 95.8 - 97.7 % |
Chromium | 0.15 - 0.35 % Show Material materials with Chromium of 0.15 - 0.35 % |
Copper | 0.1 % Show Material materials with Copper of 0.1 % |
Iron | 0.4 % Show Material materials with Iron of 0.4 % |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % |
Other | 0.15 % Show Material materials with Other of 0.15 % |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % |