AA Standards Grade 5086 H112

Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 5086 is structural alloy, which offers users strong corrosion resistance and high electrical conductivity. Offering higher strength levels than 5052 or 5083, AA 5086 becomes stronger with stain hardening and cold working, all while remaining a cost-effective choice. It can be welded with conventional methods, though electric arc welding is preferred.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H112

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Elongation

8.0 %

Show Material materials with Elongation of 8.0 %

H112

AA Standards, ASTM B209

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H112

AA Standards, ASTM B209

A100

10.0 %

Show Material materials with Elongation of 10.0 %

H112

AA Standards, ASTM B221, ASTM B241, ASTM B345

A100

12.0 %

Show Material materials with Elongation of 12.0 %

H112

AA Standards, ASTM B221, ASTM B241, ASTM B345

A50

12.0 %

Show Material materials with Elongation of 12.0 %

H112

AA Standards, ASTM B209

A100

12.0 %

Show Material materials with Elongation of 12.0 %

H112

14.0 %

Show Material materials with Elongation of 14.0 %

H112

AA Standards

A50

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 5000 Series Aluminium

Tensile strength

235.0 MPa

Show Material materials with Tensile strength of 235.0 MPa

H112

AA Standards, ASTM B209

240.0 MPa

Show Material materials with Tensile strength of 240.0 MPa

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

250.0 MPa

Show Material materials with Tensile strength of 250.0 MPa

H112

AA Standards, ASTM B209

270.0 MPa

Show Material materials with Tensile strength of 270.0 MPa

H112

AA Standards

Yield strength

95.0 MPa

Show Material materials with Yield strength of 95.0 MPa

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

RP02

105.0 MPa

Show Material materials with Yield strength of 105.0 MPa

H112

AA Standards, ASTM B209

RP02

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

H112

125.0 MPa

Show Material materials with Yield strength of 125.0 MPa

H112

AA Standards, ASTM B209

RP02

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H112

AA Standards

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

H112

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

585.0 - 640.0 °C

Show Material materials with Melting point of 585.0 - 640.0 °C

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

590.0 °C

Show Material materials with Melting point of 590.0 °C

H112

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H112

Thermal conductivity

126 W/(m·K)

Show Material materials with Thermal conductivity of 126 W/(m·K)

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

130.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 W/(m·K)

H112

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

18000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 S/m

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Electrical resistivity

5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 5.56e-08 Ω·m

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

93.0 - 96.3 %

Show Material materials with Aluminium of 93.0 - 96.3 %

H112

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Iron

0.50 %

Show Material materials with Iron of 0.50 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

0.5 %

Show Material materials with Iron of 0.5 %

H112

Magnesium

3.5 - 4.5 %

Show Material materials with Magnesium of 3.5 - 4.5 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Manganese

0.2 - 0.7 %

Show Material materials with Manganese of 0.2 - 0.7 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Other

0.15 %

Show Material materials with Other of 0.15 %

H112

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H112

AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests (O, H32, H116, H111), no damage during operation, limited damage during laboratory tests (H34, H36, H38), general: very good, without protection in industrial or seawater atmosphere

General machinability

General: poor (O, H32, H116, H111), sufficient (H34, H36, H38)

Workability

general (condition): good (O), acceptable (H32, H116, H111), poor(H36, H38)