General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 69 GPa Show Material materials with Elastic modulus of 69 GPa | |
Elongation | 23.0 °C | 8 % Show Material materials with Elongation of 8 % | |
Plane-Strain Fracture Toughnes | 23.0 °C | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m | Typical for Wrought 1000 Series Aluminium |
Poisson's ratio | 23.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium |
Shear modulus | 23.0 °C | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | Typical for Wrought 1000 Series Aluminium |
Tensile strength | 23.0 °C | 130 MPa Show Material materials with Tensile strength of 130 MPa | |
Yield strength | 23.0 °C | 110 MPa Show Material materials with Yield strength of 110 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K |
Melting point | 650 °C Show Material materials with Melting point of 650 °C | |
Specific heat capacity | 23.0 °C | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) |
Thermal conductivity | 23.0 °C | 230 W/(m·K) Show Material materials with Thermal conductivity of 230 W/(m·K) |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical conductivity | 23.0 °C | 3.30E+7 - 3.80E+7 S/m Show Material materials with Electrical conductivity of 3.30E+7 - 3.80E+7 S/m | Typical for Wrought 1000 Series Aluminium |
Electrical resistivity | 23.0 °C | 2.7E-8 - 3E-8 Ω·m Show Material materials with Electrical resistivity of 2.7E-8 - 3E-8 Ω·m | Typical for Wrought 1000 Series Aluminium |
Chemical properties
Property | Value |
---|---|
Aluminium | 99.5 - 100 % Show Material materials with Aluminium of 99.5 - 100 % |
Copper | 0 - 0.05 % Show Material materials with Copper of 0 - 0.05 % |
Iron | 0 - 0.4 % Show Material materials with Iron of 0 - 0.4 % |
Magnesium | 0 - 0.05 % Show Material materials with Magnesium of 0 - 0.05 % |
Manganese | 0 - 0.05 % Show Material materials with Manganese of 0 - 0.05 % |
Silicon | 0 - 0.25 % Show Material materials with Silicon of 0 - 0.25 % |
Titanium | 0 - 0.03 % Show Material materials with Titanium of 0 - 0.03 % |
Vanadium | 0 - 0.05 % Show Material materials with Vanadium of 0 - 0.05 % |
Zinc | 0 - 0.05 % Show Material materials with Zinc of 0 - 0.05 % |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |