General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 2.7 - 2.71 g/cm³ Show Material materials with Density of 2.7 - 2.71 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 69 - 71 GPa Show Material materials with Elastic modulus of 69 - 71 GPa | |
Elongation | 23.0 °C | 39 % Show Material materials with Elongation of 39 % | |
Hardness, Brinell | 23.0 °C | 20 [-] Show Material materials with Hardness, Brinell of 20 [-] | |
Plane-Strain Fracture Toughnes | 23.0 °C | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m | Typical for Wrought 1000 Series Aluminium |
Poisson's ratio | 23.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium |
Shear modulus | 23.0 °C | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | Typical for Wrought 1000 Series Aluminium |
Tensile strength | 23.0 °C | 65 - 95 MPa Show Material materials with Tensile strength of 65 - 95 MPa | |
Yield strength | 23.0 °C | 26 MPa Show Material materials with Yield strength of 26 MPa | |
Yield strength Rp0.2 | 23.0 °C | 20 MPa Show Material materials with Yield strength Rp0.2 of 20 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K | |
Melting point | 650 °C Show Material materials with Melting point of 650 °C | ||
Specific heat capacity | 23.0 °C | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 231 W/(m·K) Show Material materials with Thermal conductivity of 231 W/(m·K) | unstated value |
23.0 °C | 222 - 230 W/(m·K) Show Material materials with Thermal conductivity of 222 - 230 W/(m·K) | unstated value | |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical conductivity | 23.0 °C | 3.30E+7 - 3.80E+7 S/m Show Material materials with Electrical conductivity of 3.30E+7 - 3.80E+7 S/m | Typical for Wrought 1000 Series Aluminium |
Electrical resistivity | 23.0 °C | 2.82E-8 Ω·m Show Material materials with Electrical resistivity of 2.82E-8 Ω·m |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 99.5 - 100 % Show Material materials with Aluminium of 99.5 - 100 % | Balance |
Copper | 0 - 0.05 % Show Material materials with Copper of 0 - 0.05 % | |
Iron | 0 - 0.4 % Show Material materials with Iron of 0 - 0.4 % | |
Magnesium | 0 - 0.05 % Show Material materials with Magnesium of 0 - 0.05 % | |
Manganese | 0 - 0.05 % Show Material materials with Manganese of 0 - 0.05 % | |
Other | 0 - 0.03 % Show Material materials with Other of 0 - 0.03 % | Each |
Silicon | 0 - 0.25 % Show Material materials with Silicon of 0 - 0.25 % | |
Titanium | 0 - 0.05 % Show Material materials with Titanium of 0 - 0.05 % | |
Vanadium | 0 - 0.05 % Show Material materials with Vanadium of 0 - 0.05 % | |
Zinc | 0 - 0.07 % Show Material materials with Zinc of 0 - 0.07 % |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical process plant equipment, Food industry containers, Pyrotechnic powder, Architectural flashings, Lamp reflectors, Cable sheathing | |
Brazing | Excellent | |
General machinability | Poor | |
Soldering general | Excellent | |
Welding | When welding 1050 to itself or an alloy from the same subgroup the recommended filler wire is 1100. For welding to alloys 5083 and 5086 or alloys from the 7XXX series, the recommend wire is 5356. For other alloys use 4043 filler wire. Gas: Excellent; Arc: Excellent; Resistance: Excellent | |
Workability | Cold: Excellent |