General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Bending Fatigue Strength | 23.0 °C | 95 MPa Show Material materials with Bending Fatigue Strength of 95 MPa | |
Compressive modulus | 23.0 °C | 69.7 MPa Show Material materials with Compressive modulus of 69.7 MPa | |
Elastic modulus | 23.0 °C | 69 GPa Show Material materials with Elastic modulus of 69 GPa | |
Elongation | 23.0 °C | 19 % Show Material materials with Elongation of 19 % | |
Elongation A100 | 23.0 °C | 14 - 22 % Show Material materials with Elongation A100 of 14 - 22 % | |
Elongation A50 | 23.0 °C | 10 - 22 % Show Material materials with Elongation A50 of 10 - 22 % | |
Hardness, Brinell | 23.0 °C | 65 [-] Show Material materials with Hardness, Brinell of 65 [-] | 500 kg load, 10 mm ball |
Plane-Strain Fracture Toughnes | 23.0 °C | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m | Typical for Wrought 6000 Series Aluminium |
Poisson's ratio | 23.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium |
Shear modulus | 23.0 °C | 26 - 26.5 GPa Show Material materials with Shear modulus of 26 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium |
Shear strength | 23.0 °C | 165 MPa Show Material materials with Shear strength of 165 MPa | |
Tensile strength | 23.0 °C | 180 - 240 MPa Show Material materials with Tensile strength of 180 - 240 MPa | |
Yield strength | 23.0 °C | 130 MPa Show Material materials with Yield strength of 130 MPa | |
Yield strength Rp0.2 | 23.0 °C | 100 - 145 MPa Show Material materials with Yield strength Rp0.2 of 100 - 145 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 20.0 °C | 2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K |
23.0 °C | 2.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K | |
100.0 °C | 2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K | |
Melting point | 580 - 650 °C Show Material materials with Melting point of 580 - 650 °C | |
Specific heat capacity | 23.0 °C | 900 J/(kg·K) Show Material materials with Specific heat capacity of 900 J/(kg·K) |
Thermal conductivity | 23.0 °C | 155 - 180 W/(m·K) Show Material materials with Thermal conductivity of 155 - 180 W/(m·K) |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical conductivity | 23.0 °C | 2.30E+7 - 2.70E+7 S/m Show Material materials with Electrical conductivity of 2.30E+7 - 2.70E+7 S/m | Typical value |
Electrical resistivity | 23.0 °C | 3.7E-8 - 4.35E-8 Ω·m Show Material materials with Electrical resistivity of 3.7E-8 - 4.35E-8 Ω·m | Typical value |
Specific Electrical conductivity | 40 % IACS Show Material materials with Specific Electrical conductivity of 40 % IACS | Typical/Derived value |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 95.9 - 98.6 % Show Material materials with Aluminium of 95.9 - 98.6 % | |
Chromium | 0.04 - 0.35 % Show Material materials with Chromium of 0.04 - 0.35 % | |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | |
Iron | 0 - 0.7 % Show Material materials with Iron of 0 - 0.7 % | |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | |
Manganese | 0 - 0.15 % Show Material materials with Manganese of 0 - 0.15 % | |
Other | 0 - 0.15 % Show Material materials with Other of 0 - 0.15 % | each 0.05, total 0.15, Rest Al |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | |
Titanium | 0 - 0.15 % Show Material materials with Titanium of 0 - 0.15 % | |
Zinc | 0 - 0.25 % Show Material materials with Zinc of 0 - 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, T6, T651, T652, T6510, T6511), no damage during operation, limited damage during laboratory tests (T4, T451, T4510, T4511), general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), sufficient (T4, T451, T4510, T4511, T6, T651, T652, T6510, T6511) | |
Workability | general (condition): good (O), acceptable (T4, T451, T4510, T4511), poor(T6, T651, T652, T6510, T6511) |