AA Standards Grade 1060 H113

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.705 g/cm³

Show Material materials with Density of 2.705 g/cm³

H113

AA Standards, ASTM B210, ASTM B483

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H113

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H113

AA Standards, ASTM B210, ASTM B483

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

Typical for Wrought 1000 Series Aluminium

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

H113

AA Standards, ASTM B210, ASTM B483

69.0 MPa

Show Material materials with Tensile strength of 69.0 MPa

H113

Yield strength

15.0 MPa

Show Material materials with Yield strength of 15.0 MPa

H113

AA Standards, ASTM B210, ASTM B483

RP02

17.0 MPa

Show Material materials with Yield strength of 17.0 MPa

H113

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

H113

100 °C, 20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H113

AA Standards, ASTM B210, ASTM B483

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

H113

AA Standards, ASTM B210, ASTM B483

650.0 °C

Show Material materials with Melting point of 650.0 °C

H113

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H113

Thermal conductivity

230.0 - 234.0 W/(m·K)

Show Material materials with Thermal conductivity of 230.0 - 234.0 W/(m·K)

H113

AA Standards, ASTM B210, ASTM B483

230.0 W/(m·K)

Show Material materials with Thermal conductivity of 230.0 W/(m·K)

H113

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

35000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 35000000.0 - 36000000.0 S/m

H113

AA Standards, ASTM B210, ASTM B483

Electrical resistivity

2.78e-08 - 2.86e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.86e-08 Ω·m

H113

AA Standards, ASTM B210, ASTM B483

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

99.6 %

Show Material materials with Aluminium of 99.6 %

H113

AA Standards, ASTM B210, ASTM B483

99.6 - 100.0 %

Show Material materials with Aluminium of 99.6 - 100.0 %

H113

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H113

AA Standards, ASTM B210, ASTM B483

Iron

0.35 %

Show Material materials with Iron of 0.35 %

H113

AA Standards, ASTM B210, ASTM B483

0.35 %

Show Material materials with Iron of 0.35 %

H113

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H113

AA Standards, ASTM B210, ASTM B483

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

H113

AA Standards, ASTM B210, ASTM B483

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H113

AA Standards, ASTM B210, ASTM B483

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H113

AA Standards, ASTM B210, ASTM B483

Vanadium

0.05 %

Show Material materials with Vanadium of 0.05 %

H113

AA Standards, ASTM B210, ASTM B483

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H113

AA Standards, ASTM B210, ASTM B483

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12), poor (H14, H16, H18)

Workability